TechNetters:
We had that problem early on when we started to wave chip caps on the
underside of mainly through-hole CCAs. We learned from vendor's literature that
the pad width must be narrower than the chip cap width. After the artwork
change, we have not seen another chip cap crack during machine soldering.
Stu
____________________Reply Separator____________________
Subject: Re: [TN] Cracking Capacitors
Author: "FOX; Ian (York Rd)" <[log in to unmask]>
Date: 3/25/2003 5:41 PM
Joyce, thanks for that, I haven't seen that publication before. Similar
failure mode, but significantly less solder on ours than shown by TDK. We've
actually cracked them on cycling with only the build up of solder from
contact with the wave (bonded them to the surface of the PCB without
associated pads) so we aren't talking bulbous joints.
Regards
Ian
-----Original Message-----
From: joyce [mailto:[log in to unmask]]
Sent: 25 March 2003 16:38
To: 'TechNet E-Mail Forum.'; 'FOX, Ian (York Rd)'
Subject: RE: [TN] Cracking Capacitors
Seen that before... You should not use excessive solder (bending
stress)...see tdk...
http://www.component.tdk.com/components/commoncrackingmodes.pdf
jk
>-----Original Message-----
>From: TechNet [mailto:[log in to unmask]] On Behalf Of FOX, Ian (York Rd)
>Sent: Tuesday, March 25, 2003 11:37 AM
>To: [log in to unmask]
>Subject: [TN] Cracking Capacitors
>
>
>Technetters, have a little problem with capacitors that I'd be
>grateful for comments on. We've been wavesoldering 0805/1206
>chip caps onto the underside of both FR4 and poly/glass PCB's
>for the best part of 15 years and we've been experiencing a
>low failure rate of devices in-house after ESS and burn-in. On
>top of this however we've had some early life in-service
>failures. Process and assembly trials together with FEA
>analysis we've carried out suggests that the thickness of
>solder left on the topside of the device after the soldering
>operation is critical. Too much and the devices nucleate
>cracks relatively quickly, as during the negative part of the
>temperature cycle, the solders modulus increases to the extent
>that the stress imposed on the termination/body interface is
>in excess of that the titanate capacitors can withstand. My
>question to the forum therefore, is has anyone else found
>similar issues? I know we've seen posts before with regard to
>cracking caps, but this failure mode isn't anything to do with
>assembly stresses or thermal shock during the soldering
>operation (we've artificially increased the solder volume on
>convection reflow soldered components using dispensed paste
>and generated exactly the same failure
>mode)
>
>Regards
>Ian Fox
>Goodrich Engine Control Systems
>
>---------------------------------------------------
>Technet Mail List provided as a free service by IPC using
>LISTSERV 1.8e To unsubscribe, send a message to
>[log in to unmask] with following text in the BODY (NOT the
>subject field): SIGNOFF Technet To temporarily halt or
>(re-start) delivery of Technet send e-mail to
>[log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE
>mailing per day of all the posts: send e-mail to
>[log in to unmask]: SET Technet Digest Search the archives of
>previous posts at: http://listserv.ipc.org/archives Please
>visit IPC web site http://www.ipc.org/html/forum.htm for
>additional information, or contact Keach Sasamori at
>[log in to unmask] or 847-509-9700 ext.5315
>-----------------------------------------------------
>
---------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------
|
|
|