Hi Jim and Chuck,
First, the foil suppliers, I am speaking mainly of plated foil, are
definitely NOT "your best source of info. about...foils." I was the chairman
of the IPC Copper Foil committee, so I know.
Rolled and plated copper foils are 2 quite different animals. Get a copy od
IPC-TR-484 "Results of Copper Foil Ductility Round Robin Study."
Rolled Cu: E=18x10e6 psi, S depends on rolling direction and degree of
annealing [different classes], as does ductility;
Plated Cu: E~12x10e6 psi, S depends on rolling direction and degree of
annealing [different classes], as does ductility;
in both cases be aware that elongation is NOT the same as ductility; for
foils elongation is an adequate process control indicator, but is not a real
mechaniical property.
since you did not indicate what your specific interest/problem is, I cannot
give you more information.
Werner Engelmaier
Engelmaier Associates, L.C.
Electronic Packaging, Interconnection and Reliability Consulting
7 Jasmine Run
Ormond Beach, FL 32174 USA
Phone: 904-437-8747, Fax: 904-437-8737
E-mail: [log in to unmask], Website: www.engelmaier.com
---------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------
|