TECHNET Archives

February 2003

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
"TechNet E-Mail Forum." <[log in to unmask]>, "Ingemar Hernefjord (EMW)" <[log in to unmask]>
Date:
Mon, 10 Feb 2003 10:11:11 -0500
Reply-To:
Content-Transfer-Encoding:
quoted-printable
Subject:
From:
Content-Type:
text/plain; charset="iso-8859-1"
In-Reply-To:
Organization:
EXFO-TO
MIME-Version:
1.0
Parts/Attachments:
text/plain (203 lines)
Inge,
Can you do ionic extraction of your cured Ag epoxy?  If it is higher
than 40 microgram... Hmmm, what I can say...if it is 40<x<100.... Not
too bad, you should look other place.  If it is more than 100
microgram...oh, boy, you have fun...(don't forget, you need add "+" and
"-" together...Don't forget the organic complex either...hehehe).  Now,
let me ask you, did you cured stuff properly?  (how many % cure? Within
the 24 hr application of the stuff?).  
I am no Steve....Don't ask me more...
 
jk
                      
>-----Original Message-----
>From: TechNet [mailto:[log in to unmask]] On Behalf Of Ingemar 
>Hernefjord (EMW)
>Sent: Monday, February 10, 2003 9:56 AM
>To: [log in to unmask]
>Subject: [TN] Back to 97, silver migration
>
>
>Hi Techies,
>
>anyone who remember the mails that come after my lines?
>If the guys at that time (97) aren't retired and are golfing 
>and surfing in Florida, I would like to chat about the 
>headline issue, because we have seen some odd things likely. 
>My worry is about human debris (spittle) and epoxy bleeding. 
>What does saliva contain, and what's in the silver epoxy 
>bleeding remnants? Silver migration took place between Au/Ag 
>thickfilm conductors and also across MIS chips. In the later 
>case, Ag migrated from the silver epoxy, across the MIS chip 
>and climbed up on the gold bond wire. Yes,really weird.
>
>I'm not so interested in 'qualified' guessings as in 
>experiences from people around the TN. We have had a lot of 
>guessings ourselves, but need corrective actions asap.
>
>I could of cause call Mike Fenner, but he is only 0.1% of TN, 
>so there is a chance that someone more are familiar with the 
>sweet problem.
>
>Wonder what will migrate out of this?
>
>Ingemar Hernefjord
>
>Ericsson  Microwave Systems
>
>PS. Unfortunately, I don't know who 'Steve' was. Can't be 
>Steve Gregory,because he knows all secrets  himself, and is 
>teaching others.
>
>------------------------------------------------------------------
>
>teve wrote:
>>
>> All,
>>
>> Background;
>>
>> I'm being consumed by a hybrid failure suffered by one of my 
>> subcontractors. The cause of failure is silver bridging two gold 
>> conductors metallized on an alumina substrate. In DC mode, one 
>> conductor is at -5.5V, the other at +28V. The conductor spacing is 
>> ~146 microns.
>>
>> The silver is from an epoxy die attach on the +28V conductor. The 
>> silver bridging the conductors is a combination of deposited 
>> (workmanship) and dendrite (electrochemical) formation. The 
>deposited 
>> silver is half on the -5.5V wire-bond land and half bridging the 
>> alumina. Dendrites form the rest of the bridge across the alumina. 
>> Dendrites are also observed
>> *IN* the silver epoxy die attach.
>>
>> Now for the question;
>>
>> 1)Understanding the conditions necessary for silver 
>(electrochemical) 
>> migration, how could silver dendrites form *IN* the silver epoxy? 
>> There shouldn't be any potential difference *IN* silver epoxy.
>>
>> 2)How could the +28V silver migrate out of the epoxy die 
>attach across 
>> the +28V gold metallization then across the alumina? The silver die 
>> attach was completely within the +28V gold metallization. Again, no 
>> potential difference to "steer" migration. Oddly, an 
>identical config 
>> in the same hybrid did have +28V silver epoxy squeeze out into the 
>> alumina bridging 1/3 the way to -5.5V. No silver migration observed 
>> there.
>>
>> If any one can help, I can be reached @ steve.r.anderson @ trw.com 
>> (remove the spaces before & after the @).
>>
>> I can post optical & SEM/EDX images to our ftp site but they will be 
>> removed after 24 hrs.
>
>Steve
>
>
>
>------------------------------------------------------------------
>
>Silver is one of the few metals that will form "single 
>crystal" wire-like filaments when subjected to stress.  In 
>fact, in the literature, it was reported back in the '30 
>forming filaments on the same conductor/plated surface.  I 
>suspect the epoxy is expanding due to thermal stress which 
>stresses the silver and then the silver forms the filaments.
>
>Silver has always been a reliability concern inelectronic assemblies.
>
>Hope this helps.
>
>Ralph
>--
>Ralph Hersey
>
>Ralph Hersey & Associates
>3885 Mills Way
>Livermore, CA 94550-3319
>PHN: 510.454.9805
>FAX: 510.454.9805
>e-mail: [log in to unmask]
>
>----------------------------------------------------------------------
>
>Hi Steve,
>
>you`re describing interesting phenomena. Unfortunally I don`t 
>have a global answer but one (perhaps weird) idea relating to 
>your first question, how migration can take place in the 
>silver epoxy. Let try me to explain my thoughts:
>
>At first, conduction in silver filled epoxies is in principal 
>done by random contacts between the randomly placed silver 
>particles. Lets assume there are two adjacent conducting paths 
>formed by particles contacting each another, but not particles 
>of the other path (the two pathes are isolated from each 
>other). One path is at +28 V, the other one (probably short 
>and located at the edge of the conductive glue) is isolated. 
>Now lets assume migration starts and dendrites grow from the 
>-5.5 V side towards the +28V side. Where will they reach the 
>+28V side? Perhaps by chance at first at the isolated path. 
>This path then drops down to -5.5V and you`ve got two very 
>close conducting paths in the epoxy with a potential 
>difference of 33.5 V. Now one has: silver, high field 
>strength, some ionic impurities (which are resulting from the 
>chemicals used in the manufacturing of the epoxy), obviously 
>moisture - migration starts.
>
>As I understand from your mail, you got a chip land covered 
>with silver filled die attach epoxy and some bondpads very 
>close (146 micrometers seems to be unusual close to me). The 
>epoxy is sometimes squeezed out over the chip land, thus 
>reducing the distance furthermore. The first idea to reduce 
>migration issues is to get bigger distances.
>
>If, as you wrote, migration under identical build up 
>conditions in some cases took place and in others didn´t, I 
>would look carefully on moisture issues which will be probably 
>different in these cases.
>
>By the way, if you can post pictures to your ftp-side, you 
>should also be able to include them in emails. But to not 
>upset some technetters by getting megabyte big mails, if you 
>like, you could send them directly to me. I would be 
>interested in receiving them.
>
>Greetings,
>
>Ulrich Korndörfer
>
>
>----------------------------------------------------------------------
>
>---------------------------------------------------
>Technet Mail List provided as a free service by IPC using 
>LISTSERV 1.8e To unsubscribe, send a message to 
>[log in to unmask] with following text in the BODY (NOT the 
>subject field): SIGNOFF Technet To temporarily halt or 
>(re-start) delivery of Technet send e-mail to 
>[log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE 
>mailing per day of all the posts: send e-mail to 
>[log in to unmask]: SET Technet Digest Search the archives of 
>previous posts at: http://listserv.ipc.org/archives Please 
>visit IPC web site http://www.ipc.org/html/forum.htm for 
>additional information, or contact Keach Sasamori at 
>[log in to unmask] or 847-509-9700 ext.5315
>-----------------------------------------------------
>

---------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------

ATOM RSS1 RSS2