Hi Phil! I am guessing then that your components are Sn95/Pb5 in alloy
composition - if you use an aggressive flux (such as an H per JSTD-004) and
pretin the components prior to using them in assembly I would suspect that
you would have success. If the copper has migrated to the surface of the
wire finish then you will have oxidized copper/tin IMC which will be a bear
to pretin but can be accomplished. I recommend you also have confidence
that your pretinning cleaning process eliminates any "bad" residues prior
to the components going to assembly. Good Luck.
Dave
Phil Nutting
<PNutting@KAISERS To: [log in to unmask]
YSTEMS.COM> cc:
Sent by: TechNet Subject: Re: [TN] cleaning oxidized THT component leads
<[log in to unmask]>
02/26/2003 12:14
PM
Please respond to
"TechNet E-Mail
Forum."; Please
respond to Phil
Nutting
Dave,
From the manufacturer's spec sheet;
Leads... Tinned solid copper wire (medium lead content 5%)
I'm going to do some tests on solderability, both by hand and in the wave
to get a handle on production and repair solutions.
Phil
-----Original Message-----
From: Dave Hillman [mailto:[log in to unmask]]
Sent: Wednesday, February 26, 2003 11:03 AM
To: [log in to unmask]
Subject: Re: [TN] cleaning oxidized THT component leads
Hi Phil! I would echo Brian's comments about using an abrasive/mechanical
oxide removal procedure - too great of an opportunity to create
nonwetting/dewetting situations. There are a number of other chemical oxide
removal procedures (e.g. SolderNu, aggressive fluxes, acid treatments) but
realize that any chemical treatment has the potential for causing a
contamination issue of the component itself which could later be a latent
defect. What is the component finish composition - Sn63?
Dave Hillman
Rockwell Collins
[log in to unmask]
Phil Nutting
<PNutting@KAISERS To: [log in to unmask]
YSTEMS.COM> cc:
Sent by: TechNet Subject: [TN] cleaning
oxidized THT component leads
<[log in to unmask]>
02/24/2003 10:58
AM
Please respond to
"TechNet E-Mail
Forum."; Please
respond to Phil
Nutting
I have some THT capacitors that seem to have an oxide layer preventing good
solder joints. The parts were purchased about 5 years ago and are stored
loose in the stockroom bin. Aside for changing our storage habits and
polishing each lead with Scotchbrite before soldering, is there a better,
faster or easier way of cleaning the leads before soldering?
Thanks in advance for your collective wisdom.
Phil Nutting
---------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------
|
|
|