John,
We tried stripping HASL once and regretted it. The HASL coating is not
uniform in thickness. The knees of the hole wall are particularly thin. When
our captive board shop tried to strip the solder, they had to continue until
the thickest areas of solder were removed. The knees however stripped much
quicker and thus exposed the underlying copper. We ended up with problems at
the knees.
Thanks,
Robert Furrow
Printed Wiring Board Engineer
Supply Chain Networks
Lucent Technologies
978-960-3224 [log in to unmask]
-----Original Message-----
From: John Foster [mailto:[log in to unmask]]
Sent: Friday, February 14, 2003 7:12 PM
To: [log in to unmask]
Subject: [TN] question about enig
I was wondering. We just got a batch of boards that had a HASL finish when
we needed a ENIG finish. Can the HASL be stripped off and then replaced with
a ENIG finish. Our board house says no problem. But I just wanted to know
what people think. Will this be robust?
Any replies would be appreciated.
Thanks
John Foster
---------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------
|
|
|