Hi Dave,
About three years ago we did some trials on a large testboard chockfull
of fine-pitch parts. We compared a lasercut stencil and an electroformed
nickel stencil which I expected to have superior paste-release
properties.
The truth was that the lasercut stencil showed significantly better
results, with better paste-release and print definition. A process
engineer from another company told me about similar trials he had done,
with exactly the same results (he used stencils from the vendors as I
did).
Of course this doesn't say anything about the electroformed stencils
from your supplier.....
Daan Terstegge
Thales Communications
Unclassified mail
Personal Website: http://www.smtinfo.net
>>> [log in to unmask] 01/10/03 02:23pm >>>
Is anyone using electroformed stencils? We have 3 BGA 14mil apertures
and a
LLC with 16 mil we are having paste release on an auto printer. 7 hours
were
spent tweaking the print operation....separation speed, squeegee
pressure,
alignment was perfect.
We use a multi speed (vibrate) separation for paste release.
Dave Chapman
Manufacturing Engineer
Circuit Service Inc.
__________________________________________________
This message is intended for the use of the individual entity to which
it is
addressed and may contain information that is privileged, confidential
and
exempt from disclosure under applicable law. If the reader of this
message
is not the intended recipient, or the employee or agent responsible
for
delivering the message to the intended recipient, you are hereby
notified
that any dissemination, distribution or copying of this communication
is
strictly prohibited. If you have received this communication in
error,
please notify us immediately by calling
714.252.0010 or returning the original message to us. Thank You.
---------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV
1.8e
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for
additional
information, or contact Keach Sasamori at [log in to unmask] or
847-509-9700
ext.5315
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV
1.8e
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for
additional
information, or contact Keach Sasamori at [log in to unmask] or
847-509-9700
ext.5315
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV
1.8e
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for
additional
information, or contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------
|
|
|