Hi, Jean:
I think this maybe the flux emtrapment. Are you using the hand soldering process on this socket? If this like so, maybe you will use some cleanner solvents to clean the residues. But this solvents will cause the capillary and take the rosin to the socket strips!
sunny
----- Original Message -----
From: "Bissonnette, Jean-Francois" <[log in to unmask]>
To: <[log in to unmask]>
Sent: Tuesday, November 12, 2002 10:57 PM
Subject: [TN] Flux emtrapment?
I have spoted white residues under header Socket strips. It looks like
some kind of crust and some times the residues observed looked like
yellow translucent crystals.
Can this be entraped flux? I beleive so, but need to have opinion from
experts to conform.
Thanks in advance.
Jean-François Bissonnette
Vérificateur, Contrôle de la Qualité
Électronique
Produits et Procédés
Vapor Rail Inc.
10655 Henri-Bourassa O.
St-Laurent, Qc
H4S 1A1
(514) 335-4200 x2021
(514) 335-4231 fax
WABTEC CORPORATION CONFIDENTIALITY NOTE
The content contained in this e-mail transmission is legally privileged and confidential information intended only for the use of the individual or entity named herein. If the reader of this transmission is not the intended recipient, you are hereby notified that any dissemination, distribution, or copying of this transmission is strictly prohibited.
---------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------
|
|
|