Thanks all for your responses. To summarize it,
1. At -40C, material properties change, namely, much stiffer, brittle
2. At -40C, solder no creep and much stiffer
3. At -40C, delta T is larger. Delta T = -40 - Tref
Any other factors?
Yuan
-----Original Message-----
From: Zhang Tong Long [mailto:[log in to unmask]]
Sent: Tuesday, November 26, 2002 9:57 AM
To: [log in to unmask]
Subject: Re: [TN] Thermal cycling test failure modes
The -40C does kill the parts.
Let's look at the issue at component level first. At post mold cure
temperature (usually 175C), the component can be roughly considered as zero
thermal mismatch. Thermal mismatch between substrarte, silicon die and
molding compound become larger when temperature decreases.
Then let's look at the interconnect between component and PCB. it can be
roughly considered as zero thermal mismatch around 183C, when solder become
liquid. when temperature drop, thermal mismatch between component (usually
smaller effective CTE) and PCB become biger and biger.
both the stress inside the component and the stress induced due to mounting
the component on PCB increase when temperature decrease. at -40C the stress
is bigger than that at 0C and that's why you have the failures.
Hope this help.
Rgds
tonglong
-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of
[log in to unmask]
Sent: Monday, November 25, 2002 11:31 PM
To: [log in to unmask]
Subject: Re: [TN] Thermal cycling test failure modes
I think it is not the same, -40 to 85C, it is not the Delta T that kills
the parts but rather the -40C
Solder act differently at -40 compared at 0C. We are getting here the
fatigue at extreme temperatures
So it should not be the same (-40 to 85 and 0 to 125).
So Yuan, the parts interconnect could have been brittle at -40C. Trace
lay-out, board thickness, CTE's
Soldermask or Non-SMD could be a factor to that problem.
regards
Jonathan Noquil
WW Pkg Research Center
Volkmar Huss
<volkmar.huss@DRA To: [log in to unmask]
EGER.COM> cc:
Sent by: TechNet Subject: Re: [TN] Thermal
cycling test failure modes
<[log in to unmask]>
11/25/2002 11:05
PM
Please respond to
"TechNet E-Mail
Forum."; Please
respond to
Volkmar Huss
Hi Yuan,
based on what I have learned about thermal cycling tests, it is not the
low temperature that ' kills the part' but the higher delta T of 165K
compared with 125K, an increase of 32%. To prove this, you can run a
-40C to +85C profile which should have the same result as the 0C to 125C
profile.
Volkmar
Yuan Li wrote:
>
>
> We have seen some interesting phenomenaduring TCT. We compared 0-125C
> to -40- 125C. For the same package, we had no failures after 2000
> cycles with the 1st profile, but had 1st failure @ 500 cycles with the
> 2nd profile. It appears that the -40 C excursion is what kills the
> part.The most common failure we saw was substrate trace crack. The
> substrate was 2-2-2 build-up BT substrate. I know at -40C Young's
> modulus is higher. Is it a major factor? Any other factors? Why -40C
> would make sucha big difference?
>
> Recall there were some discussions on this topic, however, cannot find
> them. Any papers or on line info available?
>
> Thanks,
>
> Yuan
Volkmar Huß, C.I.D.
Engineering Electronic Circuit Boards
Aufbau- und Verbindungstechnik
_ _ _ _ _ _ _ _ _ _ _ _ _ _ _ _ _ _ _ _ _ _ _
DRÄGER ELECTRONICS
Draeger Electronics GmbH
Moislinger Allee 53-55
D-23558 Lübeck
Tel: +49-451-882-3998
Fax: +49-451-882-4365
mailto:[log in to unmask]
Website http://www.draeger-electronics.com
_ _ _ _ _ _ _ _ _ _ _ _ _ _ _ _ _ _ _ _ _ _ _
Important Notice
This email and any attachment hereto are confidential and may contain trade
secrets or may be otherwise protected from disclosure. If you have received
it in error you are in notice of this fact. Please notify us immediately by
reply email and then delete this email and any attachment from your system.
Please understand that you are not allowed to copy this email or any
attachment hereto or disclose its contents to any other person. Thank you.
---------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------
|