Glynn: Yes it's the Ni with the overplated Au that breaks off due to
excessive over etch at the interface. The result of an accelerated chemical
reaction due to larger differences in electromotive series of dissimilar
metals, as Rudy touched on. Steve never mentioned Ni in his original
question, although I would be 99% sure they are probably plating it prior to
Au.
As I stated the main objective is to control the etch process to minimize
undercut. However thicker Ni can help some if your are close to being dialed
in on the etch process, 200u" is definitely better than 30u". It also helps
to use a nickel low in organics with good ductility.
Regards
Michael Barmuta
Staff Engineer
Fluke Corp.
Everett WA
425-446-6076
-----Original Message-----
From: Glynn Shaw [mailto:[log in to unmask]]
Sent: Friday, October 11, 2002 11:43 AM
To: [log in to unmask]
Subject: Re: [TN] Undercut peeling on all Gold Board
Feel free to correct me if I'm wrong, but it is the nickel that breaks off
not the gold. The gold just comes with it, being plated over the nickel.
We've all heard of Ni-Cad batteries, well this is just a Ni-Cu battery and
the etch rate at the interface of the nickel and copper skyrockets. A
significant percentage of the time, the nickel breaks and splinters, but
does not fully detach, causing shorts from one trace to another. The only
solution is to attempt to reduce over-etching. Thicker nickel is not of
much help for this condition. It will still break off and "sliver",
regardless of thickness (within reason).
At 07:18 AM 10/11/02, you wrote:
>Steve: This is nothing new, it's inherent to the etch process with Cu/Au.
>You are getting excessive undercut and it's breaking off.
>You need tighter controls on your etching process. This includes chemical
>balance along with conveyor speed and inspection of product coming off the
>etcher. The goal is to minimize chemistry swings and exposure time in the
>etchant but still produce a complete etch.
>
>If possible 1/2oz outerlayer Cu will definitely help.
>
>Assuming you are plating Ni over the Cu prior to Au you may want to
>investigate a thicker Ni barrier plate to add support strength to the Au
>"wings" so they don't break off as easily.
>
>
>
>Regards
>
>Michael Barmuta
>
>Staff Engineer
>
>Fluke Corp.
>
>Everett WA
>
>425-446-6076
>
>
>-----Original Message-----
>From: Steve Mac Donald [mailto:[log in to unmask]]
>Sent: Thursday, October 10, 2002 1:00 PM
>To: [log in to unmask]
>Subject: [TN] Undercut peeling on all Gold Board
>
>
>Good Day to everyone,
>
>We have been experiencing an issue with deep gold plating after etch. The
>undercut is breaking away making the traces look "hairy." The gold either
>clings and drags away from the trace or breaks loose at LPI/Soldermask and
>floats in the ink to some other undesireable location. It is not consistent
>but it is persistant. Has anyone had this issue before and could someone
>suggest some possible solutions? (It never happens with standard copper
>plating--just deep gold.)
>
>Thanks,
>
>Steve MacDonald
>Mass Design
>
>---------------------------------------------------------------------------
-
>-----
>Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
>To unsubscribe, send a message to [log in to unmask] with following text in
>the BODY (NOT the subject field): SIGNOFF Technet
>To temporarily halt or (re-start) delivery of Technet send e-mail to
>[log in to unmask]: SET Technet NOMAIL or (MAIL)
>To receive ONE mailing per day of all the posts: send e-mail to
>[log in to unmask]: SET Technet Digest
>Search the archives of previous posts at: http://listserv.ipc.org/archives
>Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
>information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
>ext.5315
>---------------------------------------------------------------------------
-
>-----
>
>---------------------------------------------------------------------------
------
>Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
>To unsubscribe, send a message to [log in to unmask] with following text in
>the BODY (NOT the subject field): SIGNOFF Technet
>To temporarily halt or (re-start) delivery of Technet send e-mail to
>[log in to unmask]: SET Technet NOMAIL or (MAIL)
>To receive ONE mailing per day of all the posts: send e-mail to
>[log in to unmask]: SET Technet Digest
>Search the archives of previous posts at: http://listserv.ipc.org/archives
>Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
>information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
>ext.5315
>---------------------------------------------------------------------------
------
>
----------------------------------------------------------------------------
-----
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
----------------------------------------------------------------------------
-----
---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------
|