Blair,
We have noticed some of the same problems. I had converted our solder pots to porcelain coated crucibles. Over about a year and a half the porcelain had disintegrated. When I rebuilt it I found that the operators had cranked the temperature up into the "rapid heat" range and had cooked the crucible to a fare-thee-well. We also has some Litz wires that were fracturing after tinning when bent onto the solder posts of the next level of assembly. By running a lower temperature the brittle wire syndrome had reduced and the crucible seems to be holding up better. Naturally my operators want the large Litz wire to tin quickly so periodically they turn up the temperature, but I'm keeping a closer eye on the setting and resetting it to my desired range when I notice it is out.
I did find that there was a large buildup of gray "dust" stuck to the sides of the crucible just below the surface of the solder. With the lower temperature I'm not seeing as much of this "dust".
Phil
-----Original Message-----
From: Hogg, Blair K. [mailto:[log in to unmask]]
Sent: Wednesday, October 23, 2002 5:27 PM
To: [log in to unmask]
Subject: [TN] Dross on Solder Pot
Hello Technetters,
I'll readily admit that I'm not an expert on solder, and something has been
bothering me lately here at the shop, so I'll see what insight the forum can
yield.
We have a small solder pot used for tinning wires in our harness area.
Periodically as I walk by this pot I notice fairly thick black dross
covering the surface of the solder. This gets wiped away before they tin
wires, but lately I've noticed it turns brownish fairly quickly after wiping
off the dross from the surface.
What can be the typical causes of this? Could the pot be too hot? Could the
pot be contaminated (e.g. with copper)? Could it be contaminated because
it's too hot? I'm suggesting heat here because they run this pot at a fairly
high setting, I'm not sure why.
Thanks,
Blair Hogg
QA Manager
GAI-Tronics
---------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------
|
|
|