There is a theory in my Company that solder-filling holes, especially in
the likes of FR4 with a relatively high LCTE in the Z axis, negates the
ductility of the Cu plating inside the holes. Without the ductiity of the
plating, the risk of shearing the barrel at the interconnections with inner
layers is greatly increased with a corresponding decrease in board
reliability. I'm talking about high-rel boards here, and I subscribe to
this theory. Any thoughts, anyone?
Peter
Dave Chapman <[log in to unmask]> 30/09/2002 06:02 PM
Sent by: TechNet <[log in to unmask]>
Please respond to "TechNet E-Mail Forum."; Please respond to Dave Chapman
To: [log in to unmask]
cc: (bcc: DUNCAN Peter/Asst Prin Engr/ST Aero/ST Group)
Subject: Re: [TN] PCB design with mask over vias.
One thing we just completed was a pilot where we put apertures in our
topside SMT stencil and pasted over all vias to prevent Conformal Coat
leaking through the board. We opened the apertures +10% and got good solder
fill this also prevented corrosion or having trapped mask inside filled
vias
possible "volcano" during reflow.
Dave Chapman
Manufacturing Engineer
Circuit Service Inc.
-----Original Message-----
From: Willie Duersch [mailto:[log in to unmask]]
Sent: Friday, September 27, 2002 2:01 PM
To: [log in to unmask]
Subject: [TN] PCB design with mask over vias.
Hello Peers:
We are a CM who recently fabricated a PCBA which had the vias covered by
solder mask film design on the PCB. This is not the first time we have seen
this done in PCBA. However, in this example, the PCBA ended up inside a
refrigerator. This customer adds few notes with the PCB and nothing was
specified associated with the fab on plugging or capping of the vias. The
PCBA did not require wave solder. Aqueous clean paste was used and PCBA
washed after SMT.
The PCBA was supplied to the customer who then selectively applied
Conformal coating over the top side components on the board with a brush,
but did not coat other through holes or vias on the component side or any
area of the back side.
Over a period of time, The vias on the back side showed evidence of
corrosion and subsequent cross section analysis showed copper corrosion
from the pad part way into the barrel even under soldermask. The cross
section also showed that the LPI solder mask did not plug and did have pin
holes in the mask with bare copper in the air pockets that occur during LPI
screen deposition.
1. We feel the customer is responsible to specify the PCB and PCBA
performance criteria. Comments?
2. Is there an IPC document that covers solder mask covered vias and
guidelines associated with the practice? If not, why not?
3. Is it the PCB shop or the CM who should question, and if not
specified...should either question the practice?
4. What are the issues related to designing with solder mask film design
covered vias? In this case, the vias were .010-.014 diameter and space
constraints were not an issue. There were other holes on the PCB that were
larger diameter and were left open to coat with solder from the HASL
operation...and not coated with conformal coat.
5. What would you tell a customer to correct the issue?
There are some obvious issues and answers and I have had 12 years of
experience with PCB's. However, I really would like to have some comments
from my peers.
Best regards, Willie
----------------------------------------------------------------------------
-----
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
----------------------------------------------------------------------------
-----
---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
---------------------------------------------------------------------------------
[This e-mail is confidential and may also be privileged. If you are not the
intended recipient, please delete it and notify us immediately; you should
not copy or use it for any purpose, nor disclose its contents to any other
person. Thank you.]
---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------
|