TECHNET Archives

September 2002

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
Date:
Tue, 10 Sep 2002 09:26:12 -0500
Reply-To:
"TechNet E-Mail Forum." <[log in to unmask]>, [log in to unmask]
Subject:
MIME-Version:
1.0
Content-Transfer-Encoding:
7bit
Content-Type:
text/plain; charset=iso-8859-1
From:
Victor Hernandez <[log in to unmask]>
Parts/Attachments:
text/plain (253 lines)
Al,

   I would like to see the jpeg pictures of the suspected BGA voids.
Please provide some HISTORY of the parts to avoid confusion
Victor,

-----Original Message-----
From: [log in to unmask] [mailto:[log in to unmask]]
Sent: Tuesday, September 10, 2002 7:46 AM
To: [log in to unmask]
Subject: Re: [TN] 1mm bga voiding


Peter and Technetters,

The cross section is of a part as it comes in the door.  That part has not
been attached to a board.  The question is would the dents on the ball
cause voiding when it is reflowed.

I have also placed three additional x-section pictures of a "Reflowed"
balls.  However, I think the link requires one to sign in to ofoto.com (for
free though).

http://us.f201.mail.yahoo.com/ym/ShowLetter?YY=40492&order=down&sort=date&po
s=0&view=a&head=brief

I will email the pictures directly to anyone interested (they're in jpeg
format).

Thanks for all the replies

Al





[log in to unmask] on 09/09/2002 09:53:03 PM

To:   "TechNet E-Mail Forum." <[log in to unmask]>, [log in to unmask]
cc:   [log in to unmask]

Subject:  Re: [TN] 1mm bga voiding



Al,

You have one very irregularly shaped ball there ('skews the expression).
Can't see much of the voiding you talked about, though. I take it the bit
at the top of the picture is the component pad (?). If you are actually
getting a lot of voiding as well, I suspect that your thermal profile is a
bit hot for these components, and you may have to look at shielding them a
bit. Are these BGA's significantly smaller / less 'massive' than the other
that you say are OK? Have you tried thermocoupling these devices
specifically and taking their temperatures during the reflow cycle? What
are the results? If temp is OK, how about duration?

Peter



[log in to unmask]    10/09/2002 01:27 AM
Sent by: TechNet <[log in to unmask]>

Please respond to "TechNet E-Mail Forum."; Please respond to alan.kreplick

              To:  [log in to unmask]
              cc:  (bcc: DUNCAN Peter/Asst Prin Engr/ST Aero/ST Group)
              Subject: Re: [TN] 1mm bga voiding








Victor and other Technetters,

Hopefully this link shows the 1mm BGA picture (x-section)

http://www.ofoto.com/PhotoView.jsp?UV=922011120789_31499403105&US=0&collid=2
9888403105&photoid=19888403105




Al




Victor Hernandez <[log in to unmask]>@IPC.ORG> on 09/09/2002
12:23:59 PM

Please respond to "TechNet E-Mail Forum." <[log in to unmask]>; Please respond
      to [log in to unmask]

Sent by:  TechNet <[log in to unmask]>


To:   [log in to unmask]
cc:

Subject:  Re: [TN] 1mm bga voiding


Al,

   The IPC-A-610C sec. 12.2.12 Area Array/Ball Grid Array states that "
Acceptable - Class 1,2,3 Less than 10% voiding in the ball to board
interface.   Process Indicator - Class 2,3  10-25% voiding in the ball to
board interface.   What is the SIZE of the ball you are using.

   Did we have to SIGN UP to the Web Page to view your photo.   Perhaps a
fellow TechNetter can offer their site for viewing.

victor,

-----Original Message-----
From: [log in to unmask] [mailto:[log in to unmask]]
Sent: Monday, September 09, 2002 9:13 AM
To: [log in to unmask]
Subject: [TN] 1mm bga voiding


Technetters-

We are getting 1mm BGA devices with these mechanical defects (see attached*
for link to picture) from testing processes at the vendor.

These devices have excessive voiding when reflowed on to a board with other
BGAs that do not have a voiding problem.  The vendor insists it is our
process that causes the voiding.

Question-  would you expect this mechanical damage to lead to voiding in
the reflowed joint?


*
http://www.ofoto.com/ShareLandingSignin.jsp?UV=922011120789_31499403105&US=0



&Upost_signin=OrderPhotos.jsp%3FshowSlide%3Dtrue&Un=774560513&Um=54718403105



.84079403105



Al

----------------------------------------------------------------------------



-----
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
----------------------------------------------------------------------------



-----

----------------------------------------------------------------------------
-----



Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
----------------------------------------------------------------------------
-----



----------------------------------------------------------------------------
-----


Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
----------------------------------------------------------------------------
-----






[This e-mail is confidential and may also be privileged. If you are not the
intended recipient, please delete it and notify us immediately; you should
not copy or use it for any purpose, nor disclose its contents to any other
person. Thank you.]

----------------------------------------------------------------------------
-----
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
----------------------------------------------------------------------------
-----

---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------

ATOM RSS1 RSS2