Peter,
In our experience bridging occurs because the BGA warps ("pancakes") during
reflow. Wrap is induced by CTE mis-matches between the materials in the
package. We investigated this problem in depth by conducting a series of
designed experiments. Here is what we found:
1. Use a baffled nozzle
2. Minimize air flow rates
3. Maintain temperature on top of BGA package at < 220C
4. Minimize time above reflow beyond supplier recommendation
We pay very close attention to the above when generating profiles to rework
plastic BGAs that are > 35mm. The bigger the BGA and the finer the pitch,
the more prone they become to bridging at the corners. Some parts have such
a narrow process window that we down-graded them to non-preferred status.
I'll be glad to discuss in more detail. Contact me offline.
Tom Buschor, Harris Corp.
Melbourne, Florida
---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------
|
|
|