Yes, the parts (components, not boards) are made in Asia.
Just call me Bev. Mr. Christian sounds too "Mutiny on the Bountish". :)
Bev Christian
Research in Motion
-----Original Message-----
From: Rudy Sedlak [mailto:[log in to unmask]]
Sent: July 24, 2002 3:00 PM
To: [log in to unmask]
Subject: Re: [TN] Need info on a material
Mr. Christian:
Suspect that the fabricator may not be rinsing the parts well after
application of the juice.
They apply hot....if the parts dry between the application and the rinses,
and the rinses are cold....this could spell a problem.
I assume that you are using boards made in Asia?
Rudy Sedlak
RD Chemical Company
----------------------------------------------------------------------------
-----
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
----------------------------------------------------------------------------
-----
-----Original Message-----
From: Bev Christian
Sent: July 24, 2002 2:14 PM
To: 'TechNet E-Mail Forum.'
Subject: RE: [TN] Need info on a material
:)
I am on the receiving end of this one, Rudy. We do not make the parts, but
are receiving them and we are wondering if this material is why we are
having solderability problems, i.e. it is not "getting out of the way" of
the molten solder front as it wets across the lead. When we take the parts
and sonicate them in IPA and then test them they do MUCH better.
regards,
Bev Christian
Research in Motion
-----Original Message-----
From: Rudy Sedlak [mailto:[log in to unmask]]
Sent: July 24, 2002 11:57 AM
To: [log in to unmask]
Subject: Re: [TN] Need info on a material
Mr. Christian:
You called sir?
You called it exactly, this juice is an OSP type product.
When you have porous Gold plating on top of Nickle, any exposed Nickle sets
up a galvanic cell, and tends to oxidize/corrode more quickly than if it
were exposed without being in contact with Gold. This stuff reacts with the
exposed Nickle, and renders it less reactive...it is actually a very elegant
idea, because it will only react with exposed Nickle (contrary to their
website) thus the possibility of there being ANY effect on conductivity is
virtually nil.
Now, is this really an issue? Am I missing an opportunity? I wouldn't want
my fellow Techneters to have to import this stuff from Japan...and I am
always ready to assist whenever I can.. I can already see the name....ONP
BC "Organic Nickle Protection....as suggested by Bev Christian.
Rudy Sedlak
RD Chemical Company
----------------------------------------------------------------------------
----- Technet Mail List provided as a free service by IPC using LISTSERV
1.8e To unsubscribe, send a message to [log in to unmask] with following text
in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet
NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send
e-mail to [log in to unmask]: SET Technet Digest Search the archives of
previous posts at: http://listserv.ipc.org/archives Please visit IPC web
site http://www.ipc.org/html/forum.htm for additional information, or
contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
----------------------------------------------------------------------------
-----
---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------
|