Hi Patti,
What you have is most likely a combination of the large ceramic/FR-4 thermal
expansion mismatch causing cyclic creep-fatigue and tensile displacements
frozen-in during hand-soldering causing creep rupture.
"More ductile solder" is not a solution. More uniform soldering and lower
thermal expansion mismatch strains are; the latter can be accomplished by
more compliant lead geometries, and if that is not possible, to a lesser
extent by an increased stand-off to increase solder joint thickness.
Werner Engelmaier
Engelmaier Associates, L.C.
Electronic Packaging, Interconnection and Reliability Consulting
7 Jasmine Run
Ormond Beach, FL 32174 USA
Phone: 386-437-8747, Fax: 386-437-8737
E-mail: [log in to unmask], Website: www.engelmaier.com
---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------
|
|
|