TECHNET Archives

June 2002

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Content-Transfer-Encoding:
quoted-printable
Sender:
Subject:
From:
Charles Caswell <[log in to unmask]>
Date:
Tue, 4 Jun 2002 13:07:54 -0500
Content-Type:
text/plain; charset="iso-8859-1"
MIME-Version:
1.0
Reply-To:
"TechNet E-Mail Forum." <[log in to unmask]>, Charles Caswell <[log in to unmask]>
Parts/Attachments:
text/plain (68 lines)
Watch out for rubber bands around those silver immersion boards. Ours came in clear poly bags with rubber bands around each stack of ten. Result, black line across the top and bottom board in each bundle. Wiped off easly enough on most of them, but a couple had to be scrapped.
Charles Caswell
Process Lead, PCB
 Frontier Electronic Systems

-----Original Message-----
From: [log in to unmask] [mailto:[log in to unmask]]
Sent: Tuesday, June 04, 2002 11:20 AM
To: [log in to unmask]
Subject: Re: [TN] Oxidation problem in Silver plated components leads


Brian Ellis suggests:

What you are seeing is probably not oxidation but sulfidation. Trace
quantities of SO2 or H2S in the air will cause this. Other than the
aesthetic view, light sulfidation is harmless and reasonable flux
activity should be sufficient to handle it. The best way of prevention
is controlled atmosphere storage.

Doug chimes in:

I would agree with Brian.  Recently, Dave Hillman and I looked over an
immersion silver board that had black traces around the edges of the board,
and in one case, the whole back side of the board.  The board had been
wrapped with silver saver paper.  When I did some ion chromatography work
on the black residue, I found that it was high in both chloride and sulfur.
The silver saver paper was relatively low in both materials, but it had
been taped closed using normal masking tape and put inside a polyethylene
bag.  Analyzing the tape itself with a relatively benign extraction, we
found that it was loaded with both chloride and sulfur.  This was not very
surprising as most tape adhesives are loaded with these two material.  It
is my theory that the masking tape outgassed sulfur (or chloride) and so
tarnished the boards.  Unfortunately, I have not had the time (or funding)
to nail this down, but it does track with some of my experiences at CSL.

On the other hand, Dave analyzed the black material using SERA (where Dave
is the undisputed master) and SERA said the black material was silver
chloride.

This begs larger questions, what is your storage environment, what is your
storage material set (e.g. silver saver paper in polyethylene bags).

Doug Pauls
Rockwell Collins

---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------

---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------

ATOM RSS1 RSS2