Hi, Michael,
I use Dexter's FP6100 (Dexter is now part of Loctite), which is a capillary
action type underfill applied after everything else has been assembled and
tested. I chose it for a number of reasons, notwithstanding the fact that
it requires the board to be heated to around 90 deg C while carrying out
the underfilling process, and further heated at 150 deg C for 10 minutes to
cure it afterwards:
1. FP6100 is reworkable at normal soldering/desoldering temperatures, which
'no-flow' type underfills are not.
2. FP6100 does not have to be applied at time of assembly, so if a BGA
fails test, it is easier and cleaner to replace.
3. It does not limit me to the flux contained in a 'no-flow' - I follow the
normal assembly process using our espatblished choice of flux.
4. It does come off quite cleanly when de-soldering and removing an
underfilled BGA, and residues can be removed with a solder wick when
cleaning up the BGA site for the replacement component. A final clean with
alcohol before fitting a new component and the site is prepared.
IMHO, there is no problem with using a capillary type underfill, apart from
requiring the extra process and thermal excursion forthe board, but to me,
it's benefits outweigh these disadvantages.
Peter
"WEEKES, MICHAEL HS-SNS" <[log in to unmask]> 15/05/2002 10:35 PM
To: "'TechNet E-Mail Forum.'" <[log in to unmask]>, DUNCAN
Peter/Asst Prin Engr/ST Aero/ST Group@ST Domain
cc:
Subject: RE: [TN] BGA's on ruggedized assemblies...
Is underfill really reworkable - I know rework may be feasible, but let's
be
honest about the detrimental effects of the thermal effect and
contamination
of a site where underfill was applied, cured, heated and
mechanically/chemically removed. I welcome comment - our assemblies are
too
expensive to scrap out. Any personal experience with any loctite or other
"reworkable" undefilled - I rank "reworkable" up there with "washable, but
not soluble".
-----Original Message-----
From: [log in to unmask] [mailto:[log in to unmask]]
Sent: Tuesday, May 14, 2002 8:01 PM
To: [log in to unmask]
Subject: Re: [TN] BGA's on ruggedized assemblies...
Our Rockwell friends, through the fumes of Mountain Dew and Coke, will say
"No" if your attachment processes are good enough. Personally, though,
after some early (low level) vibration failures with some third party
designed and assembled boards, I built some more to my own spec and
introduced underfilling as an insurance policy. I hope to be able to
vibration qual test boards with and without underfilling to see if this
process is really necessary.
To answer your question, it depends .... on your processes, the operating
conditions and expected life of the product, and maybe even the board and
BGA materials. Underfill manufacturers claim that using underfill can
improve the fatigue life of BGA solder joints by a factor between 3 and 5,
but it is another process and it involves heating boards an extra time (if
you use the capillary action type underfill) to carry out the underfill
process and cure the material. The no-flow type is applied and cured
concurrently with the assembly of the BGA onto the board and doesn't
involve the extra thermal excursion.
I recommend you try qualifying boards with underfill and without it to see
if you need the extra process. Underfilling is not necessary in all
situations, nor a recommendation, but it won't do any harm either if you
want to use it anyway.
Peter
[log in to unmask] 15/05/2002 05:08 AM
Sent by: TechNet <[log in to unmask]>
Please respond to "TechNet E-Mail Forum."; Please respond to SteveZeva
To: [log in to unmask]
cc: (bcc: DUNCAN Peter/Asst Prin Engr/ST Aero/ST Group)
Subject: [TN] BGA's on ruggedized assemblies...
Hi All!
Gotta question, when BGA's are used on ruggedized assemblies (at least
Level-4, probably Level-5), is underfilling BGA's recommended, or a
necessity?
Thanks, as always...
-Steve Gregory-
[This e-mail is confidential and may also be privileged. If you are not the
intended recipient, please delete it and notify us immediately; you should
not copy or use it for any purpose, nor disclose its contents to any other
person. Thank you.]
----------------------------------------------------------------------------
-----
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send e-mail to [log in to unmask]:
SET
Technet NOMAIL
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
----------------------------------------------------------------------------
-----
[This e-mail is confidential and may also be privileged. If you are not the
intended recipient, please delete it and notify us immediately; you should
not copy or use it for any purpose, nor disclose its contents to any other
person. Thank you.]
---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------
|