Hi, Antonio,
As the other two respondants have indicated, voids in BGA joints are
principally caused by volatile compounds in the flux out-gassing into the
joint. Voids in these cases tend to be small and of no significance as long
as they don't blow out through the side of the ball, which is rare. Larger,
more irregularly-shaped voids can occur when you have via holes in the
pads, unfilled holes especially, although these holes are normally plugged
nowadays.
Voids in BGA joints are common and are not considered to be a problem
unless they are very large and/or found at the top of the ball next to the
compnoent substrate. These weaken the balls' adherence to the component.
Careful selection of flux and tight soldering process control can eliminate
voiding, but the cost of this will be high with no real advantage gained
unless your voids are a problem.
Best wishes
Peter
Antonio Souza
<[log in to unmask] To: [log in to unmask]
INPE.BR> cc: (bcc: DUNCAN Peter/Asst Prin Engr/ST
Sent by: Aero/ST Group)
TechNet Subject: [TN] Voids on BGA
<[log in to unmask]
ORG>
04/10/02
08:25 PM
Please
respond to
"TechNet
E-Mail
Forum.";
Please
respond to
Antonio Souza
Does anybody know the main causes for Voids on BGA solder joints?
Thanks
Antonio
Brazil
---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send e-mail to [log in to unmask]:
SET Technet NOMAIL
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
---------------------------------------------------------------------------------
[This e-mail is confidential and may also be privileged. If you are not the
intended recipient, please delete it and notify us immediately; you should
not copy or use it for any purpose, nor disclose its contents to any other
person. Thank you.]
---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------
|
|
|