Hi Wm. Dean May! I recommend that you look at your 1010 steel problem from
a different perspective. No solder alloy will wet to 1010 steel unless you
activate the 1010 surface with an applicable flux. Soldering to steel
typically requires a very "active" flux (e.g IPC-JSTD-004 type H) which, if
not properly removed, can lead to corrosion later in life. I recommend
talking with the flux vendors (e.g Kester, Alpha, Indium, ESP, etc) to get
their recommendation for an appropriate flux and cleaning procedure. Once
you are able to wet the 1010 surface then you need to decide what solder
alloy to use - are you looking for solderability, mechanical strength, high
temperature stability, etc.? - you can see where I am going with this. Good
Luck.
Dave Hillman
Rockwell Collins
[log in to unmask]
"May William D (Dean) CNIN" <[log in to unmask]>@ipc.org> on
04/08/2002 08:47:37 AM
Please respond to "TechNet E-Mail Forum." <[log in to unmask]>; Please respond
to "May William D (Dean) CNIN" <[log in to unmask]>
Sent by: TechNet <[log in to unmask]>
To: [log in to unmask]
cc:
Subject: [TN] Solder alloy for 1010 Steel
We have some 1010 cold rolled steel board stiffeners that require soldering
to a circuit card like a through-hole part. Does anyone know if there are
any solder alloys that will wet to 1010 steel? We could have them
electroplated with tin/lead to make them solderable but was curious if
there
was an alternative.
Thanks for your consideration!
Wm. Dean May
NSWC Crane
Bldg. 38, Code 6086
300 Highway 361
Crane, IN 47522
812-854-3073
---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send e-mail to [log in to unmask]:
SET Technet NOMAIL
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search previous postings at: www.ipc.org > On-Line Resources & Databases >
E-mail Archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
---------------------------------------------------------------------------------
---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/scripts/wa.exe?S1=technet
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------
|
|
|