Lupita,
Listen to your suppliers! My previous company had immersion tin
as a final surface finish, which I was directly involved and after
several months of trying to determine your same question I would
say that 6 months is tops especially if you take into consideration
if the board you are assembling is multiple pass through wave
solder. All of this testing/evaluation was performed using SERA
(sequential electromigration reduction analysis) and at the time
evaluating the three biggest players Dexter, Omikron, and
McGean Rohco.
Tony Steinke
----- Original Message -----
From: Lupita Roberts <[log in to unmask]>
To: <[log in to unmask]>
Sent: Wednesday, March 20, 2002 8:34 AM
Subject: [TN] FW: shelve life of pwb's
> I am wondering if anyone can help me with the shelve life of raw
> PWB's. I was experiencing solderability issues and oxidation issues
> with some boards. I was told by several suppliers that White Tin only
> has a shelve life of 6 months and they were not warrantied beyond that
> point. I have been unsuccessful in trying to find data in regards to
> this issue.
>
> Suzanne Foulkes
> QC Supervisor
> Inservco Inc.
> LaGrange, Ohio 44050
>
> [log in to unmask]
> [log in to unmask]
>
> --------------------------------------------------------------------------
-------
> Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt delivery of Technet send e-mail to [log in to unmask]:
SET Technet NOMAIL
> To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
> Search previous postings at: www.ipc.org > On-Line Resources & Databases >
E-mail Archives
> Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
> information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
> --------------------------------------------------------------------------
-------
---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------
|
|
|