text/plain (79 lines)
Earl,
I sympathize with you on this problem because we have also seen similar
situations with ENIG finishes.  We a particular board which is mixed
technology board (SMT and thru hole) and there is one thru hole connector
area in particular that consistently exhibits poor wetting.  The entire rest
of the board wets fine, SMT and thru hole.  This connector area has pads
tied into heavy ground planes and they typically don't wet.  In a simple
minded model, it  seems like the gold dissolves into the solder before the
nickel reaches wetting temperature, thus the nickel becomes passsivated?
Any ideas.
Jim Kittel


-----Original Message-----
From: Earl Moon [mailto:[log in to unmask]]
Sent: Monday, March 11, 2002 4:57 AM
To: [log in to unmask]
Subject: Re: [TN] ENIG AND NON WETTING


Daan,

As always, I appreciate your input. To clarify, the boards were freshly
received from a major international supplier. I instructed our assembly
house (the same major international supplier - how about that for strategic
planning as the same boards, in volume will be, guess what, assembled by the
same major international supplier in another location) to reflow and wave
solder the solder samples. The supplier wave soldered the side in which I
had little interest. It was the SMT side, with all the little bastard TI
CSP's that held the most interest for obvious reasons or that should have
been obvious to all as it's all I've been yacking about for two months to
you all and all prospective suppliers.

I got the wave results last week with the non wetting as I described. The
wave solder process was "normal" to the major international assembly
operation with flux type, flux application, conveyor speed, wave types, wave
height, preheat temps, solder temp, and all the other stuff we all know and
love about wave soldering and its process management requirements.

The board showed, clearly, non wetting on some bottom side SMT pads, at
about 50% non wetted. It also showed, clarly through hole pads about 50%, by
quantity, non wetted with some obviously adhacent.

My question, again, is what in the ENIG, over bare copper after SM
application, is possibly affecting this type solderability. It's a mystery
worth more investigation.

Again, thanks Daan and I hope I clarified.

Earl

----------------------------------------------------------------------------
-----
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search previous postings at: www.ipc.org > On-Line Resources & Databases >
E-mail Archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
----------------------------------------------------------------------------
-----

---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives