Hi Jim! A simple way to understand the impact of a conditioning cycle on a
solder joint is to think of the two dominate failure phenomena - creep and
fatigue. Creep is a time dependent strain under a given stress (e.g. apply
a load and the solder joint crack grows over time) and fatigue is solder
joint crack resulting from a repeated or fluctuating stress which is less
than the solder alloy tensile strength (e.g. apply a repetitive load and
the solder joint cracks grows in relation to the stress cycles). If solder
behaved like steel then life would be pretty mundane and a bunch of us
metallurgical engineers would be looking for work! However, solder joint
microstructure changes just sitting at room temperature. Depending on how
you apply stress and how you apply temperature you can get either creep or
fatigue or both interacting thus understanding how the solder joint crack
is progressing very tough (this is the focus area where Guenter, Werner,
and many other folks have spent thousands of hours attempting to understand
which mechanisms are dominate for a given conditioning recipe). The rate of
change of a conditioning recipe has a direct impact on dominate failure
mode - that's why trying to mimic your use environment conditions with a
conditioning cycle can be important. Hope this helps.
Dave Hillman
Rockwell Collins
[log in to unmask]
"Marsico, James" <[log in to unmask]>@ipc.org> on 03/11/2002 05:56:07
AM
Please respond to "TechNet E-Mail Forum." <[log in to unmask]>; Please respond
to "Marsico, James" <[log in to unmask]>
Sent by: TechNet <[log in to unmask]>
To: [log in to unmask]
cc:
Subject: Re: [TN] Thermal Shock
Glenn (or anyone else), could you elaborate on your statement that slow
rates of change affect solder joints more than fast rates of change.
Thanks,
Jim Marsico
Senior Engineer
Production Engineering
EDO Electronics Systems Group
[log in to unmask] <mailto:[log in to unmask]>
631-595-5879
-----Original Message-----
From: Pelkey, Glenn [SMTP:[log in to unmask]]
Sent: Friday, March 08, 2002 3:27 PM
To: [log in to unmask]
Subject: Re: [TN] Thermal Shock
Hi Nancy,
Question 1:
Thermal Shock has some room for interpretation, but in
general, it is a high rate of temperature change. When I say high, I mean
greater than 30 C/min. Even within the mil specs there is some confusion:
Mil-Std-883, Method 1010 is termed "Temperature Cycling" and requires less
than 1 minute transfer time between extremes. However, a similar test
method in Mil-Std-202, Method 107 is termed "Thermal Shock" and allows up
to
5 minutes transfer time. Other Thermal Shock test methods use liquid as
the
medium of heat exchange rather than air, but I'm assuming you're using air.
Question 2:
If the failure mechanism from the Thermal Shock test is the
same as would be expected in the field, then there is an Acceleration
Factor
you can use to relate the two. Just do an internet search for
"Coffin-Manson" for the equation or let me know if you need further
help...I
can set you up a quick spreadsheet. However, the key is same failure
mechanism. As pointed out by others in this group, most soldered
assemblies
experience slow rates of change, which affect solder joints more than fast
rates of change. But, your end use environment may be different.
Question 3:
I'm not sure what you're asking here. Can you elaborate?
Glenn
-----Original Message-----
From: Nancy Trumbull [ mailto:[log in to unmask]
<mailto:[log in to unmask]> ]
Sent: Friday, March 08, 2002 5:40 AM
To: [log in to unmask]
Subject: [TN] Thermal Shock
Hi Everyone,
It has been awhile for me. I have had so much work that I've
had no time to take part in Technet. So please forgive me.
My Question :
1)What is the equivalent of a Thermal shock cycle?
2) How do I evaluate a failure if it fails with-in 80 cycles?
3) How do I break down a cycle so it would pretain to the
part?
The cycle we have been told to use and evaluate our parts with is
the following:
160 cycles
At -30°C ½ hr ® + 80°C ½ hr
If needed this is an assembled board.
As it is now I can only say it passed or it failed. I can not say
how long the part will last, good or bad.
I have looked in IPC Test Method book TM-650 but could not find any
thing.
Well if any one has any thing let me know. If not I thank each and
every one of you for your time.
Have a good week end.
Nancy T.
----------------------------------------------------------------------------
-----
Technet Mail List provided as a free service by IPC using LISTSERV
1.8d
To unsubscribe, send a message to [log in to unmask] with following
text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search previous postings at: www.ipc.org > On-Line Resources &
Databases > E-mail Archives
Please visit IPC web site http://www.ipc.org/html/forum.htm
<http://www.ipc.org/html/forum.htm> for additional
information, or contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
----------------------------------------------------------------------------
-----
---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send e-mail to [log in to unmask]:
SET Technet NOMAIL
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search previous postings at: www.ipc.org > On-Line Resources & Databases >
E-mail Archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
---------------------------------------------------------------------------------
---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------
|