Go to laminate suppliers as polyclad, Nelco, etc. Each has its list of glass
styles and resin contents, etc.
Please note, the need for homogenious materials. You can ask what that means
but examples are 2113, 2116, 1080.
As examples, 2113 is about 4 mils thick with a resin content of about 58$.
2116 is about 5 mils thick with a resin congent of about 53%. 1080 is about
2.5 mils thick with a resin content from 65 to 70$. Also include 106 as a
homogeneous glass style (60 yarn bundles per inch, made up of 7-9 micron
glass fibers, in the warp direction - and I'll explain why this is important
when asked)
I'll give you MY chart of materials, resin contents, if you wish, and usage
requirements that have served me well over many years.
Earl
---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------
|
|
|