Hello Siggi,
We had the same problem,
1) Using HASL finish to the board will not help you because as Brain Ellis
said the amount of solder that drains down the via is much more then you
supply (coat + print )- we tried it without success.
2) DO not Mask the Vias from the bottom side it will cause very big voids.
3) You can try to seal the vias with paste but note that if it will have
height it can cause problem during printing.
4) I recommend you to use blind microvias or just take the holes out of the
pads.
Regards,
Marki Sasportas.
-----Original Message-----
From: Zweigart, Siegmund [mailto:[log in to unmask]]
Sent: Tuesday, March 05, 2002 9:53 AM
To: [log in to unmask]
Subject: Re: [TN] Via in Pad? Need Help!!!
Hello Ken
We had the same problem (or still have).
We tried HASL and OCC Boards but there was no difference.
We also tried plugging with a special stencil and 63/37 but this don't
works.
We did not try a high temperature solder.
Masking is quite critical because of voids.
Beside redesign you have only one chance: Look for new process parameters.
Siggi
----------
From: Ken Patel [SMTP:[log in to unmask]]
Sent: Montag, 4. März 2002 23:37
To: [log in to unmask]
Subject: [TN] Via in Pad? Need Help!!!
Importance: High
Guys,
On our nickel gold board, solder joints are below IPC spec
(insufficient
solder) where there are vias in pad. Solder is drained down the via
holes and deprived the joint of necessary solder. I would like to
know
the following.
(1) How about using the surface finish 63/37 coating HASL instead of
Ni-Gold? I think gold dissolves in solder so quickly that I rather
use
HASL processed boards, any thoughts?
(2) Do you guys mask the via on bottom side to avoid solder draining
out
on the other side?
(3) Does anybody try Hi Temp solder paste to fill the vias as our
assembly house ordered via stencils to fill the via using eutectic
(63/37) solder paste which didn't work?
Looking for
re,
Ken Patel
----------------------------------------------------------------------------
-----
Technet Mail List provided as a free service by IPC using LISTSERV
1.8d
To unsubscribe, send a message to [log in to unmask] with following
text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search previous postings at: www.ipc.org > On-Line Resources &
Databases > E-mail Archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for
additional
information, or contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
----------------------------------------------------------------------------
-----
----------------------------------------------------------------------------
-----
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search previous postings at: www.ipc.org > On-Line Resources & Databases >
E-mail Archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
----------------------------------------------------------------------------
-----
---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------
|
|
|