TECHNET Archives

February 2002

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Content-type:
text/plain; charset=us-ascii
Sender:
Subject:
From:
Date:
Fri, 1 Feb 2002 17:34:34 +0800
MIME-Version:
1.0
X-To:
Reply-To:
"TechNet E-Mail Forum." <[log in to unmask]>, [log in to unmask]
Parts/Attachments:
text/plain (100 lines)
Mike,

It looks like you have exceeded the plugging criteria on two practical
counts - 1) is that your aspect ratio is too high (6:1 is deemed to be the
limit a hole can be filled to and 2) is that all the fab houses I've talked
with who are experienced with the plugging process baulk at filling holes
smaller than 12 mils and that's with a 4:1 aspect ratio.

I can't say for sure what's happening to your boards, but I would hazzard a
serious guess (given the circumstances) that the VIA plug has been unable
to outgas properly, and since the epoxy has cured, there is nowhere now for
trapped gasses to escape to.

If possible, open out your holes to 15 mils and have a serious word with
your fab house to see if they truly understand the VIA plugging process.
Outgassing the material properly prior to filling, especially for small
diameter/high aspect ratio holes, is of prime importance. I've used this
process on quite a few boards now, and only has two troublesome episodes -
both at start-up with a new fab house, where plating adhesion wasn't as
good as it should have been.

Hope this matches one of your favourite theories.

Peter




                    Michael.Forrester@
                    LECROY.COM                To:     [log in to unmask]
                    Sent by: TechNet          cc:     (bcc: DUNCAN Peter/Asst Prin Engr/ST
                    <[log in to unmask]>         Aero/ST Group)
                                              Subject:     [TN] Dupont CB100  VIA Plug and
                                              Delamination
                    02/01/02 08:28 AM
                    Please respond to
                    "TechNet E-Mail
                    Forum."; Please
                    respond to
                    Michael.Forrester






We have been having a problem with Dupont silver CB100 VIA Plug.  The
boards are 12 layer, .062", FR4, Nickel/Gold plated.
We have a BGA pattern with VIA in hole.  The VIAs are filled with CB100 VIA
plug and then the board is plated.
The VIAs are .010 causing an aspect ratio of 6.2:1.  We are seeing after
solder reflow, inner layer delamination in the area of the
VIA filled BGA patterns.  Has anyone seen this before?  Does anyone use a
similar construction and had success?  There are a few
theories flying around but I wanted to ask the IPC community for any
insight.  Thank you in advance.

Best Regards,

Mike Forrester
Sr. Manufacturing Engineer
[log in to unmask]

---------------------------------------------------------------------------------

Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send e-mail to [log in to unmask]:
SET Technet NOMAIL
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search previous postings at: www.ipc.org > On-Line Resources & Databases >
E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for
additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
---------------------------------------------------------------------------------





[This e-mail is confidential and may also be privileged. If you are not the
intended recipient, please delete it and notify us immediately; you should
not copy or use it for any purpose, nor disclose its contents to any other
person. Thank you.]

---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------

ATOM RSS1 RSS2