Peter,
If you have the space to do it, I would suggest increasing the pad size to
about 0.265" square, or, if not, reducing the clip contact area
correspondingly so that you can obtain heel, toe and side solder fillets.
Without these, you are producing stress concentration points that will in
turn cause low peel strength.
Peter
Peter Lee
<ppwlee@YAHOO To: [log in to unmask]
.COM> cc: (bcc: DUNCAN Peter/Asst Prin Engr/ST
Sent by: Aero/ST Group)
TechNet Subject: [TN] Pull strength on soldered clip
<[log in to unmask]
ORG>
02/09/02
04:17 PM
Please
respond to
"TechNet
E-Mail
Forum.";
Please
respond to
Peter Lee
Hello,
I ran into an application requiring SMT reflow soldering of a small
copper clip to a pad. The resulting solder joint was so weak that a
slight pull on the overhanging lip will rip off the entire clip from the
pad. I examined the mating surfaces afterwards and both were still
solderable.
The 0.005" thick clip has a flat 1/4"x1/4" surface which was placed
right on top of the pad with the same size. Stencil aperture is 1:1 and
both the pad and clip have good solderability (before and after). The
rest of the components on the boards are soldered well. I like to know
if there is a way to determine how much pull strength should I expect
with such design? In order to strengthen the solder joint, does it make
sense to increase the size of the pad to ensure wetting on the edge and
force excess solder to flow on top of the clip?
Any advice is appreciated.
Rgds,
Peter
_________________________________________________________
Do You Yahoo!?
Get your free @yahoo.com address at http://mail.yahoo.com
---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send e-mail to [log in to unmask]:
SET Technet NOMAIL
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search previous postings at: www.ipc.org > On-Line Resources & Databases >
E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for
additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
---------------------------------------------------------------------------------
[This e-mail is confidential and may also be privileged. If you are not the
intended recipient, please delete it and notify us immediately; you should
not copy or use it for any purpose, nor disclose its contents to any other
person. Thank you.]
---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------
|
|
|