TECHNET Archives

January 2002

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
Subject:
From:
TOE /Torben Østeraa <[log in to unmask]>
Date:
Wed, 30 Jan 2002 15:15:30 +0100
Content-Type:
text/plain; charset="ISO-8859-1"
MIME-Version:
1.0
Reply-To:
"TechNet E-Mail Forum." <[log in to unmask]>, TOE /Torben Østeraa <[log in to unmask]>
Parts/Attachments:
text/plain (130 lines)
Adam,

You may also be inspired by this article:

http://www.circuitree.com/CDA/ArticleInformation/features/BNP__Features__Ite
m/0,2133,24954,00.html

regards

Torben Oesteraa
Printca AS


-----Original Message-----
From: Robert Peterson [mailto:[log in to unmask]]
Sent: Wednesday, January 30, 2002 1:47 PM
To: [log in to unmask]
Subject: Re: [TN] pulse plating - without additives


Hi,
I've never done it, but there is an article available at
http://dynatronix.com/copper.html

Hope this helps

Bob Peterson
Alternate Final Finishes, Inc.

-----Original Message-----
From: Adam Seychell [mailto:[log in to unmask]]
Sent: Wednesday, January 30, 2002 3:10 AM
To: [log in to unmask]
Subject: [TN] pulse plating - without additives


Hello platers.  I am hoping someone here can share a few words
of wisdom about reverse pulse plating. I'm having difficulty
finding detailed information on the subject, as my local university
library showed to carry almost nothing. It seems  that the
literature on reverse pulse plating is bound to research papers
only (which I latter learned can be quite costly and time
consuming to obtain). What I like to know is a method of plating
"standard" printed circuit boards in acid copper bath *without*
the use of additives. Pulse plating without additives has been
done or so I've been told, however most documents I have
read only talk about baths containing additives.

Normally, a pure DC in acid copper (200 g/l H2SO4, 20 g/l Cu)
would produce a rough and grainy deposit, especially when
thickness' become high ( >35 um). The problem is aggravated by
 increasing current density. Even at current densities of
0.5A/dm2 the deposits still remain unacceptable. This is
something I have observed through experimentation.

A test panel was plated using reverse pulse technique to see
what effect it had compared to DC plating at an equivalent
average current density. Not having a proper pulse plating power
supply I constructed my own basic one, using standard DC supply
and an electronic circuit to periodically reverse the output. The
parameters of the plating were:

forward time = 5 ms
reverse time = 1.7 ms
forward & reverse current densities = 3 A/dm2
average current density = 1.5 A/dm2

The pulse plating deposits were only slightly improved over DC
plating. A rough and crystalline surface was clearly visible under a
40X microscope. This does not sound promising and I am hoping
this is due to incorrect characteristics of the current pulse. Most
reverse pulse plating systems tend to use forward/reverse current
ratios of around 3, forward times of 10~20ms and reverse times
1~2ms. Is important for the current reverse pulse to be short and
high ?

If anyone could guide me to right path I'd be greatly thankful. If
there is no such thing as additive free copper plating for PC
fabrication then kindly let me know as this could save me lot of
time doing what others have already attempted.

regards,

Adam Seychell.

----------------------------------------------------------------------------
-----
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search previous postings at: www.ipc.org > On-Line Resources & Databases >
E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
----------------------------------------------------------------------------
-----

----------------------------------------------------------------------------
-----
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search previous postings at: www.ipc.org > On-Line Resources & Databases >
E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
----------------------------------------------------------------------------
-----

---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------

ATOM RSS1 RSS2