Hi Neal! I am just guessing but the problem may be using 100 grams to
measure a 50 mil thick plating layer - get a copy of the ASTM E384 and ASTM
E18 specifications - the restrictions/requirments for test load versus
plating thickness should be listed. Good Luck.
Dave Hillman
Rockwell Collins
[log in to unmask]
"Neel, Robert" <[log in to unmask]>@ipc.org> on 01/15/2002
12:16:59 PM
Please respond to "TechNet E-Mail Forum." <[log in to unmask]>; Please respond
to "Neel, Robert" <[log in to unmask]>
Sent by: TechNet <[log in to unmask]>
To: [log in to unmask]
cc:
Subject: [TN] Nickel Plating Snarl
Folks,
Can someone explain to me why all my PCB houses are suddenly having
"spectacular cows" over this pcb plating spec:
"CONTACT PATTERN FINISH IS ELECTROLESS NICKEL, 50 MILLIONTHS THICK, MINIMUM
40 ROCKWELL C HARDNESS, MEASURED WITH KNOOP PROCESS @ 100 GRAMS"
This pcb is the substrate for some snap-acting domes and I need a hard and
conductive bearing surface for the dome feet. The plating spec comes from
the dome manufacturer.
Is it the "electroless"? Is it the thickness? Is it the hardness
requirement? Is it the "nickel" vs "nickle"? (Funny thing is, though,
everyone is very happy to do gold rather than nickel.)
What gives?
Robert
---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------
|
|
|