TECHNET Archives

December 2001

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Content-Transfer-Encoding:
7bit
Sender:
Subject:
From:
David Douthit <[log in to unmask]>
Date:
Tue, 4 Dec 2001 09:57:59 -0700
Content-Type:
text/plain; charset=us-ascii; x-mac-type="54455854"; x-mac-creator="4D4F5353"
MIME-Version:
1.0
Reply-To:
"TechNet E-Mail Forum." <[log in to unmask]>
Parts/Attachments:
text/plain (68 lines)
OOPPPPS!!!!

I suppose the best I can say about this is that the water film would be thicker, form sooner,
and the temperature/humidity combination is closer to real world conditions.

I have been taught that the film thickness at which the water begins to act chemically the
same as bulk water is 5 molecules. As the temperature increases it requires higher levels of
humidity to reach this thickness with all other things being equal.

David A. Douthit
Manager
LoCan LLC

[log in to unmask] wrote:

> David Douthit exclaims:
>
> First; trying to grow dendrites in a 85/85 environment is difficult at
> best. Dendrites
> require liquid water. the free energy at 85 degrees C is to high. It will
> not allow a liquid
> water film to form. you must be below 40 degrees C to ensure the formation
> of liquid water.
>
> Doug Pauls, well into his second Mt. Dew of the day, responds:
> No it doesn't, no it doesn't, no it's not, yes it will, and no you don't,
> respectively.
>
> It is not hard to grow dendrites, I do it frequently.  Anyone who does SIR
> testing will say the same.  I've even grown dendrites on gold samples.
> Dendritic growth takes moisture, bias and an ionic contaminant.  The
> greater the magnitude of these factors, the greater the propensity for
> dendritic growth.  Yes, most dendritic growth requires liquid water, but
> you only need a few molecular thicknesses to do this, which is easily
> attained at 85/85.  Yes, liquid water can form at 85/85.  All you need is a
> 1-2 degree difference in temperature between the environment and your
> substrate and poof, water.   When water forms, temperature wise, depends on
> the relative humidity and the temperature.  SIR testers, if they have done
> it long enough, have had an occasion where power goes out on the chamber
> and the temperature drop while the humidity remains high.  You rapidly
> reach the dew point well above 40C.
>
> I'm sure Brother Ellis in Cyprus can expound on the physics in greater
> depth.
>
> Doug Pauls
> Rockwell Collins
>
> ---------------------------------------------------------------------------------
> Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt delivery of Technet send the following message: SET Technet NOMAIL
> Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives
> Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
> information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
> ---------------------------------------------------------------------------------

---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send the following message: SET Technet NOMAIL
Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------

ATOM RSS1 RSS2