Etch conditions for Kovar are pretty much the same as Copper with Ferric
Chloride.
A lot of the small houses etch Iron based alloys first with Ferric Chloride,
then finish up etching Copper.
Usually you use 40+ Baume' Ferric Chloride, and the key issue is watching the
HCl, you keep it low to give you good "etch ratios", and higher to increase
speed.
Rudy Sedlak
RD Chemical Company
---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send the following message: SET Technet NOMAIL
Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------
|
|
|