Hi, Steve,
I've had a number of ENIG boards made, and they don't look THAT rough.
Looks like someone's run a blunt drill through the board very fast.
Problems? - apart from "Are the holes cleaned and conditioned properly for
plating in the first place?":
Ductility of the copper, or at least its ability to stretch as much as it
could in the Z, perhaps.
Reliability of interconnection between layers?
Local delam behind the plating if the drill did have a rough ride?
Dunno.
Do you have any test coupons exhibiting the same phenomenon to cross
section?
Peter Duncan
"Stephen R.
Gregory" To: [log in to unmask]
<SteveZeva@AO cc: (bcc: DUNCAN Peter/Asst Prin Engr/ST
L.COM> Aero/ST Group)
Sent by: Subject: [TN] Rough PTH barrel walls in ENIG
TechNet plated PCB...
<[log in to unmask]
ORG>
11/21/01
06:38 AM
Please
respond to
"TechNet
E-Mail
Forum."
Hi all!
Just recieved a bare fab that I noticed some very rough walls of the
barrels of the PTH's. This is a ENIG plated PCB by the way. The roughness
seems worse in the smaller diameter holes than do the larger holes. Go to:
http://www.stevezeva.homestead.com/
and look at the two pics titled "rough walls"...
Didn't see any real voids, or fibers protruding...just maybe this is the
way ENIG always plates, and it's just the way it always looks down inside
holes, I've never noticed it being this rough before...See any problems?
Thanks!
-Steve Gregory-
[This e-mail is confidential and may also be privileged. If you are not the
intended recipient, please delete it and notify us immediately; you should
not copy or use it for any purpose, nor disclose its contents to any other
person. Thank you.]
---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send the following message: SET Technet NOMAIL
Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------
|
|
|