Stephen,
In our HALS equipment this is daily routine.This daily treatment takes 3
hours.
We are running also solder analysis 3 times a month with very consistent
results.Apart of daily treatment solder composition corrections are very
rare.As you mentioned,from time to time we have to add some pure tin.
Edward

Edward Szpruch
Eltek , Manager of Process Engineering
P.O.Box 159 ; 49101 Petah Tikva Israel
Tel  ++972 3 9395050 , Fax  ++972 3 9309581
e-mail   [log in to unmask]

> -----Original Message-----
> From: Stephen S. Schiera [SMTP:[log in to unmask]]
> Sent: в аевеси 14 2001 18:46
> To:   [log in to unmask]
> Subject:      Re: [TN] Solder analysis results
> 
> You will want to take another sample after doing this.  As you cool the
> pot
> the heavier metals (i.e. lead) will drop.  When you remove the dross you
> will be removing tin also and could change the Sn/Pb ratio.  You can buy
> pure tin to add back in to correct this.
> 
> -----Original Message-----
> From: Edward Szpruch [mailto:[log in to unmask]]
> Sent: Tuesday, August 14, 2001 11:35 AM
> Subject: Re: Solder analysis results
> 
> 
> Phil,
> Copper content is 5.5 times higher that should be.
> Try to remove the excess copper by veeery slow cooling of your solder pot
> in
> static conditions.Around 190 centigrade you should get the first dross on
> the surface ,which is very rich in copper.Take it out.
> Good luck
> Edward
> 
> Edward Szpruch
> Eltek , Manager of Process Engineering
> P.O.Box 159 ; 49101 Petah Tikva Israel
> Tel  ++972 3 9395050 , Fax  ++972 3 9309581
> e-mail   [log in to unmask]
> 
> > -----Original Message-----
> > From: Phil Nutting [SMTP:[log in to unmask]]
> > Sent: в аевеси 14 2001 14:48
> > To:   [log in to unmask]
> > Subject:      [TN] Solder analysis results
> >
> > Ok folks, here is today's question.
> >
> > I just received a Certificate of Analysis (our first one) for the solder
> > in our Soltec Waver Solder machine.  All parameters are "within
> > specification" except the percentage of copper which is at 1.6859. (Tin
> > is at 61.3% and Lead is at 36.99% and other stuff is at 0.0199%)  We run
> > 63/37 in the wave.  We only solder our own product, none of which goes
> > into "mission critical" applications.  We normally build our product to
> > IPC-A-610C, Class 2.
> >
> > My question is two-fold.  Should I worry about this?  If so, how do I
> > fix it with 1700 pounds of solder in the solder pot?
> >
> > Thanks is advance for sharing your knowledge.
> >
> > Phil Nutting
> > Manufacturing Engineer
> > Kaiser Systems, Inc.
> >
> >
> --------------------------------------------------------------------------
> > -------
> > Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
> > To unsubscribe, send a message to [log in to unmask] with following text
> in
> > the BODY (NOT the subject field): SIGNOFF Technet
> > To temporarily halt delivery of Technet send the following message: SET
> > Technet NOMAIL
> > Search previous postings at: www.ipc.org > On-Line Resources & Databases
> >
> > E-mail Archives
> > Please visit IPC web site (http://www.ipc.org/html/forum.htm) for
> > additional
> > information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
> > ext.5315
> >
> --------------------------------------------------------------------------
> > -------
> 
> --------------------------------------------------------------------------
> -------
> Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt delivery of Technet send the following message: SET
> Technet NOMAIL
> Search previous postings at: www.ipc.org > On-Line Resources & Databases >
> E-mail Archives
> Please visit IPC web site (http://www.ipc.org/html/forum.htm) for
> additional
> information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
> ext.5315
> --------------------------------------------------------------------------
> -------

---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send the following message: SET Technet NOMAIL
Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------

---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send the following message: SET Technet NOMAIL
Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------

ATOM RSS1 RSS2