Hi Darrel,
I have worked for a flex circuit manufacturer for about a decade. The
procedures for soldering flex are about the same as soldering other more
conventional substrates. You will want to bake the flex in an oven at approx
100 degrees F for at least an hour prior to assembly. Kapton is hygroscopic
and this will drive out any moisture absorbed by the kapton. You will also
want to try to complete the soldering operation in the shortest time
possible. You will not want to dwell on the flex for long.
Hope this helps.
Christopher Lampron
-----Original Message-----
From: Darrel Therriault [mailto:[log in to unmask]]
Sent: Sunday, September 30, 2001 9:27 PM
To: [log in to unmask]
Subject: [TN] Flex and Soldering
Technet,
Does anyone have any guidelines for soldering flex circuit directly to a
PWB? We currently connect it mechanically and with a connector, but
were toying with the idea of direct solder attach.
Any experience, do's and don't, especially horror stories, appreciated.
Thanks......DT
--
Darrel Therriault
VP, Mfg. Operations
INCEP Technologies, Inc
(858)547-9925 223
[log in to unmask]
----------------------------------------------------------------------------
-----
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send the following message: SET
Technet NOMAIL
Search previous postings at: www.ipc.org > On-Line Resources & Databases >
E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
----------------------------------------------------------------------------
-----
---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send the following message: SET Technet NOMAIL
Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------
|
|
|