I would guess that 7781 is the yarn type, and E-glass is the standard glass
type used for FR-4 and most rigid PCB laminate materials.
According to Electronic Packaging Materials and Their Properties (Pecht et
al.), E-glass is 54.5% SiO2, 14.5-15-2% Al2O3, 17.2% CaO, 4.7% MgO, 8.0%
B203 and smaller amounts of some other compounds. Has a dielectric constant
of 6.3, density of 2.54 g/cc, CTE of 5.5 ppm/C. There is also S-glass,
D-glass, and quartz--all less common.
I don't see 7781 listed as a yarn type, but I do see 55.51, 5111, 5221,
6331, 7221, 9681 and 9991. I think the number relates to the number of glass
strands and how they are spun together.
Tim Reeves
-----Original Message-----
From: Steve Telgen [mailto:[log in to unmask]]
Sent: Friday, August 10, 2001 8:52 AM
Subject: Material specification
Hi, everyone,
Does anyone know what 7781 E glass is? It's supposed to be a type of
fiberglass material for PCBs.
TIA
Steve Telgen
IGK Industries
---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send the following message: SET Technet NOMAIL
Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------
|