Hi, Joyce,
I am talking from an avionics standpoint. Minor measling is acceptable, but
if there are any concerns about further delamination from the measles, they
can be 'lanced' and injected with resin to bond them.
Pete Duncan
Joyce Koo
<jkoo@RESONANCE-PHOT To: [log in to unmask]
ONICS.COM> cc: (bcc: DUNCAN Peter/Asst Prin Engr/ST Aero/ST Group)
Sent by: TechNet Subject: Re: [TN] Measling...
<[log in to unmask]>
06/05/01 08:34 PM
Please respond to
"TechNet E-Mail
Forum."; Please
respond to Joyce Koo
I am no so sure...Steve is using polyimide board, which most likely is
for high reliability usage (not off the shelf items for commercial
usage)...I would not use it if it is for avionics (measling cross the
sky is scary...it may infect the stars...)..jk
-----Original Message-----
From: <Peter George Duncan> [mailto:[log in to unmask]]
Sent: June 4, 2001 10:23 PM
To: [log in to unmask]
Subject: Re: [TN] Measling...
No. The measling looks quite minor and doesn't come close to other
traces
or pads. Unless I'm mis-judging the scale of the picture, the affected
area
isn't carrying high power either, so I don't see that there's a problem.
Pete Duncan
"Stephen R.
Gregory" To: [log in to unmask]
<SteveZeva@AO cc: (bcc: DUNCAN Peter/Asst
Prin Engr/ST Aero/ST Group)
L.COM> Subject: [TN] Measling...
Sent by:
TechNet
<[log in to unmask]
ORG>
06/05/01
02:58 AM
Please
respond to
"TechNet
E-Mail
Forum.";
Please
respond to
SteveZeva
Hi ya'll!
I took a few days off last week, and came back to be confronted with
some
boards that have been measled from rework...
Go to: http://stevezeva.homestead.com/index.html to take a peek.
The boards are polyimide, and it obviously appears that there was too
much
heat used when they were reworked...also they may have not been baked
prior
to the rework...I was told that they were, but you know how that goes.
I know what the -610 says about it, it says it's acceptable as long as
the
assembly performs as specified. There isn't any burns or anything around
any
of the barrels, just the measles...and it's only on one 14-pin DIP
location.
Would any of you have any REAL hesitation about accepting this assembly?
Thanks!
-Steve Gregory-
------------------------------------------------------------------------
---------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send the following message: SET
Technet NOMAIL
Search previous postings at: www.ipc.org > On-Line Resources & Databases
> E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for
additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
------------------------------------------------------------------------
---------
---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send the following message: SET
Technet NOMAIL
Search previous postings at: www.ipc.org > On-Line Resources & Databases >
E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for
additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
---------------------------------------------------------------------------------
---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send the following message: SET Technet NOMAIL
Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------
|
|
|