TECHNET Archives

June 2001

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Content-Transfer-Encoding:
quoted-printable
Sender:
Subject:
From:
"Bissonnette, Jean-Francois" <[log in to unmask]>
Date:
Tue, 19 Jun 2001 12:53:38 -0400
Content-Type:
text/plain; charset="iso-8859-1"
MIME-Version:
1.0
Reply-To:
"TechNet E-Mail Forum." <[log in to unmask]>, "Bissonnette, Jean-Francois" <[log in to unmask]>
Parts/Attachments:
text/plain (117 lines)
Thank you all for your answers.  That confirms a lot of speculations.  Only
one
question remains:  Can this affect the reliability of the coating and have
long
terms effects?  Since it seems that moisture vapor is condensed into the
coating,
I guess that yes, but for those who faced this situation before, were you
able to
use the boards in this condition without problems?

Thanks again!

Jean-François Bissonnette

> -----Original Message-----
> From: Alan Brewin [mailto:[log in to unmask]]
> Sent: Tuesday, June 19, 2001 4:28 AM
> To: TechNet E-Mail Forum.; Bissonnette, Jean-Francois
> Subject: Re: [TN] Conformal coating: white haze
> 
> 
> Jean Francois,
> 
> Blushing is generally caused by high humidity.  It is usually 
> worst in spray
> applications, but can become an issue in dipping/brushing 
> applications as
> well.
> 
> Essentially, as the solvent starts to flash-off, the 
> evaporation causes
> cooling (cf. acetone on your hand!), which then causes some 
> of the saturated
> moisture vapour to be condensed onto and into the coating.  
> Atomisation
> causes more cooling and hence greater problems with blushing.
> 
> You could try adding a retarder solvent, but a much better 
> solution would be
> to try and reduce your humidity.  You could try using a portable
> de-humidifier and held-held probe to try and maintain a max 
> RH of about 60%,
> but aim for 40%.
> 
> Hope this helps,
> 
> Best Regards,
> 
> Phil Kinner
> (Masquerading as Alan Brewin!)
> 
> ----- Original Message -----
> From: Bissonnette, Jean-Francois
> To: [log in to unmask]
> Sent: 18 June 2001 16:35
> Subject: [TN] Conformal coating: white haze
> 
> 
> This is a question for all the conformal coating specialists of this
> world.
> 
> We're experiencing some problems with the application of 
> conformal coating
> in high humidity
> conditions.  Just after the application is finished, some 
> kind of white haze
> appears in the coating.
> It disappears a little be during curing but some of it stays. 
>  The finish of
> the coating is then a little
> less smooth and shinny than normal.
> 
> In order to avoid excess of humidity, the boards are 
> pre-heated for 24h.
> The coating used is
> acrylic.
> 
> Anyone knows what causes this?
> 
> 
> Jean-François Bissonnette
> Contrôle de la Qualité, Électronique
> Quality Control, Electronics
> Vapor Canada Inc.
> 10655 Henri-Bourassa O.
> St-Laurent, Qc
> H4S 1A1
> (514) 335-4200 Ext: 2021
> 
> 
> 
> WABTEC CORPORATION CONFIDENTIALITY NOTE
> The content contained in this e-mail transmission is legally 
> privileged and
> confidential information intended only for the use of the 
> individual or
> entity named herein. If the reader of this transmission is 
> not the intended
> recipient, you are hereby notified that any dissemination, 
> distribution, or
> copying of this transmission is strictly prohibited.
> 


WABTEC CORPORATION CONFIDENTIALITY NOTE
The content contained in this e-mail transmission is legally privileged and confidential information intended only for the use of the individual or entity named herein. If the reader of this transmission is not the intended recipient, you are hereby notified that any dissemination, distribution, or copying of this transmission is strictly prohibited.

---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send the following message: SET Technet NOMAIL
Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives