Hi Ed: Take a close look and see if the discoloration is only on the mask or
is it also on the laminate in the exposed area around the pads. If it is on
both it could possibly be the flux being over baked during preheat and the
wetter being left behind causing a hazy appearance. If it is just on the
mask, it's probably that the very top resin portion on the surface of the
mask has broken down and exposed some of the filler in the mask. The
DSR-3241 is a semi-matte to matte style of mask that uses quite a bit of
filler to create its appearance.
Have you checked the cure to verify that the mask is fully
cured/crosslinked. Insufficient cure both thermal and UV can contribute to
this problem.
I'm also assuming you are seeing this only on the board bottom side i.e.
flux/solder side and before any cleaning operation.
Regards
Michael Barmuta
Staff Engineer
Fluke Corp.
Everett WA
425-446-6076
-----Original Message-----
From: Ed Hare [mailto:[log in to unmask]]
Sent: Wednesday, May 23, 2001 10:12 AM
To: [log in to unmask]
Subject: [TN] Discoloration of LPI solder mask
Dear Technetters,
Thanks in advance for any insight you can offer on this issue ...
The issue is discoloration of LPI solder mask (ENPLATE DSR-3241 (MD)) that
corresponds to areas that were selectively wave soldered I believe using OA
flux. There are pictures at the link below ...
http:\\www.eskimo.com\~ehare\EH_516
The discoloration does not map with ground planes or other internal
circuitry in the PWB.
What might cause this type of discoloration?
Thanks,
Ed Hare
SEM Lab, Inc.
----------------------------------------------------------------------------
-----
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send the following message: SET
Technet NOMAIL
Search previous postings at: www.ipc.org > On-Line Resources & Databases >
E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
----------------------------------------------------------------------------
-----
---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send the following message: SET Technet NOMAIL
Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------
|
|
|