Steve,
I have seen that before with conventional glob-topped assemblies if: They
had been subjected to thermal cycling; solder reflow (a thermal cycle); had
poor adhesion to the substrate for one reason or another; selected a poor
choice of encapsulant material (TCE mis-match); were improperly cured
(allowed to sit at room humidity for a long time before heat cure); or a
combination of all of the above.
PS - the parts that I built, did not exhibit this anomaly, but Brand-X's
did!
Regarding Non-technical content - I can find my Delete key. It is not a big
deal. I have too many other problems arising during the course of the day
to fret about such things. To some extent we DO need to be somewhat
tolerant/considerate of others. If cracking a joke eases the stress, so be
it - as long as one considers it to be in good taste, and is in moderation.
Back to my skulking in the shadows.
Steve Creswick
-----Original Message-----
From: Stephen R. Gregory [mailto:[log in to unmask]]
Sent: Tuesday, May 08, 2001 5:39 PM
To: [log in to unmask]
Subject: [TN] Removing Epoxy Encapsulation...
Hi ya'll!!
Thanks for all the suggestions for chemicals to remove epoxy encapsulation
material.
I had some Uresolve 411 here, but that won't work. Our customer has sent
some
parts to a failure analysis lab, and the vendor is doing some work on their
end too.
I was looking at the parts under a microscope holding it with tweezers, and
was gently scraping it with an x-acto knife, when the whole encapsulation
just popped off! It wasn't any force at all!
I got a few more parts and found that I could very easily separate the whole
glob off with hardly any force at all...like the encapsulation material
wasn't bonded well to the substrate. I took a picture, go to:
http://stevezeva.homestead.com/index.html
You see the wire in the epoxy, and the silver epoxy for the die...but as you
can see, the whole deal popped of very cleanly...are you supposed to be able
to do that? Any ideas?
-Steve Gregory- <----Flak jacket is on in case he slips and makes a
joke...hehehe
----------------------------------------------------------------------------
-----
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send the following message: SET
Technet NOMAIL
Search previous postings at: www.ipc.org > On-Line Resources & Databases >
E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
----------------------------------------------------------------------------
-----
---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send the following message: SET Technet NOMAIL
Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------
|
|
|