Ioan,
Are you absolutely sure your wave is stable - no weird up and down
variations?
Have you confirmed no organics on the pads prior to soldering via FTIR or
Auger or simply washing the boards thoroughly before running them?
Have you used a wetting balance or SERA tester to check the
solderability/oxide amount on the pads that did not solder?
regards,
Bev Christian
Research in Motion
-----Original Message-----
From: Tempea, Ioan [mailto:[log in to unmask]]
Sent: April 6, 2001 12:25 PM
To: [log in to unmask]
Subject: [TN] Random absence of solder joints - update
Hi technos,
and big thanks for the interest in my problem. Now, I tried to follow all
the leads, I checked the solder mask, I ruled out the contamination, since
the problem shows on each and every board, checked for oily residues, etc.
To clarify, the problem pads show no sign of having been in contact with the
solder, they are like before waving.
So I still can't put the finger on the cause. However, by hand spraying the
bottoms, or running the foam fluxer at max, we reduced the number of
problems. We even get, from time to time, fully soldered boards.
Maybe the boards have gone through some thermal cycling that made the
intermetallics grow, or the pads are oxidized for some reason. Maybe a bad
batch. I'm sure that a stronger flux would solder very well, but why this
deviation from the regular process, since we are talking regular boards?
So, the follow up question is:
what should I do to avoid that the problem reappear while running a future
job, eventually high volume?
Thanks,
Ioan
----------------------------------------------------------------------------
-----
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send the following message: SET
Technet NOMAIL
Search previous postings at: www.ipc.org > On-Line Resources & Databases >
E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
----------------------------------------------------------------------------
-----
---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send the following message: SET Technet NOMAIL
Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------
|