Good idea to use more of the original solder mask for touch up - but a couple
of further pointers to help make your life easier.
1. If the original mask is LPI - it is cured with both a photo exposure and a
bake. Doubt an assembly shop has UV light of that intensity - so really
watch the bake - don't short cut that. The bake at touch-up has to cure as
much as combined expose and bake at original fab. Also, be sure this extra
bake is not damaging any surface finish conditions - OSP, immersion tin or
silver, or forming extra copper/tin intermetallic from the tin/lead solder of
a HASL board. If original mask was dry film - you obviously have to use a
different liquid mask for touch up.
2. Lots of mask formulations come as two part - resin and catalyst. You have
to get both parts from your board fab, and then you have a mixed mask pot
life of a few hours. Mix no more than you will use quickly in the touch-up
operation. Likewise, most masks are carried in solvent. Some solvent may
evaporate from your mixed resin/catalyst, so get some extra solvent from your
fab shop. Or, you may want to make a more dilute mask formulation to be able
to brush-on touch up areas more easily.
3. If you don't like these complications, you might consider touching up
with a one part thermal cure mask from the old days. That stuff is pretty
simple.
Denny Fritz
MacDermid, Inc.
---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send the following message: SET Technet NOMAIL
Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------
|
|
|