TECHNET Archives

April 2001

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
"Ingemar Hernefjord (EMW)" <[log in to unmask]>
Date:
Tue, 24 Apr 2001 08:02:32 +0100
Reply-To:
Mike Fenner <[log in to unmask]>
Subject:
MIME-Version:
1.0
Content-Transfer-Encoding:
7bit
Content-Type:
text/plain; charset="Windows-1252"
From:
Mike Fenner <[log in to unmask]>
Parts/Attachments:
text/plain (202 lines)
Stannum

Mike

----- Original Message -----
From: "Ingemar Hernefjord (EMW)" <[log in to unmask]>
To: <[log in to unmask]>
Sent: Tuesday, April 24, 2001 7:31 AM
Subject: Re: [TN] Embrittlement


> another one falling into #2 is me. Gold is Aurorum, Silver is
Argentum, Lead is Plumbum, but what was Sn? Was it Senilium? /Ingemar
>
> -----Original Message-----
> From: Wenger, George M (George) [mailto:[log in to unmask]]
> Sent: den 23 april 2001 19:46
> To: [log in to unmask]
> Subject: Re: [TN] Embrittlement
>
>
> Bev,
> It's only a tough question if 1). You didn't have a metallurgy
course or 2).
> you start to get old and forgetful.  I didn't take #1 but I know a
lot about
> #2.  I think Dave, like the rest of us, is starting to fall into #2.
>
> I think he meant to tell you AuSn4 and AgSn3 not Au4Sn and Ag3Sn
>
> Regards,
> George
> George M. Wenger, DMTS Bell Laboratories Princeton
> Supply Network Solutions
> PO Box 900, Princeton NJ 08542-0900
> Route 569 Carter Rd., Hopewell, NJ 08525
> (609)-639-2769 (Office), 3210 (Lab), 2346 (Fax)
> [log in to unmask]
>
>
> -----Original Message-----
> From: David Hillman [mailto:[log in to unmask]]
> Sent: Monday, April 23, 2001 12:54 PM
> To: [log in to unmask]
> Subject: Re: [TN] Embrittlement
>
>
> Hi Bev! There is a fairly large set of industry data on the solder
joint
> reliability problems induced by Gold/Tin intermetallic  (Au4Sn)
formation
> and a smaller data set on the solder joint reliability problems
induced by
> Silver/Tin intermetallic  (Ag3Sn) formation.  See Klein Wassink's
book ISBN
> 0-901150-24-X. I would expect that if you have both intermetallic
species
> in a solder joint it just would not be a "good" thing. The use
environment
> of the assembly would also play a role in just "how much"
intermetallic
> degradation would be allowable. Tough question - good luck.
>
> Dave Hillman
> Rockwell Collins
> [log in to unmask]
>
>
>
>
> Bev Christian <[log in to unmask]>@IPC.ORG> on 04/16/2001 08:33:58
AM
>
> Please respond to "TechNet E-Mail Forum." <[log in to unmask]>; Please
respond
>       to Bev Christian <[log in to unmask]>
>
> Sent by:  TechNet <[log in to unmask]>
>
>
> To:   [log in to unmask]
> cc:
>
> Subject:  [TN] Embrittlement
>
>
> Good morning!
> Here is a met. question to start off the day.
>
> We know that if we have over 4% gold in a 63/37 tin lead solder
joint we
> risk gold induced embrittlement because of the production of a
significant
> amount of the tin/gold intermetallic.  It is also common practise to
use a
> slight variation of the eutectic solder with a 62/36/2 Sn/Pb/Ag
> composition.
> We also know that gold and silver are 100% soluble in each other.
My
> question: if the final tin/lead based solder joint composition has a
> COMBINED noble metal percentage in the 4% range how bad is that for
solder
> joint reliability?
>
> regards,
> Bev Christian
> Research in Motion
>
> --------------------------------------------------------------------
--------
> -----
>
> Technet Mail List provided as a free service by IPC using LISTSERV
1.8d
> To unsubscribe, send a message to [log in to unmask] with following
text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt delivery of Technet send the following message:
SET
> Technet NOMAIL
> Search previous postings at: www.ipc.org > On-Line Resources &
Databases >
> E-mail Archives
> Please visit IPC web site (http://www.ipc.org/html/forum.htm) for
> additional
> information, or contact Keach Sasamori at [log in to unmask] or
847-509-9700
> ext.5315
> --------------------------------------------------------------------
--------
> -----
>
> --------------------------------------------------------------------
--------
> -----
> Technet Mail List provided as a free service by IPC using LISTSERV
1.8d
> To unsubscribe, send a message to [log in to unmask] with following
text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt delivery of Technet send the following message:
SET
> Technet NOMAIL
> Search previous postings at: www.ipc.org > On-Line Resources &
Databases >
> E-mail Archives
> Please visit IPC web site (http://www.ipc.org/html/forum.htm) for
additional
> information, or contact Keach Sasamori at [log in to unmask] or
847-509-9700
> ext.5315
> --------------------------------------------------------------------
--------
> -----
>
> --------------------------------------------------------------------
-------------
> Technet Mail List provided as a free service by IPC using LISTSERV
1.8d
> To unsubscribe, send a message to [log in to unmask] with following
text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt delivery of Technet send the following message:
SET Technet NOMAIL
> Search previous postings at: www.ipc.org > On-Line Resources &
Databases > E-mail Archives
> Please visit IPC web site (http://www.ipc.org/html/forum.htm) for
additional
> information, or contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
> --------------------------------------------------------------------
-------------
>
> --------------------------------------------------------------------
-------------
> Technet Mail List provided as a free service by IPC using LISTSERV
1.8d
> To unsubscribe, send a message to [log in to unmask] with following
text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt delivery of Technet send the following message:
SET Technet NOMAIL
> Search previous postings at: www.ipc.org > On-Line Resources &
Databases > E-mail Archives
> Please visit IPC web site (http://www.ipc.org/html/forum.htm) for
additional
> information, or contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
> --------------------------------------------------------------------
-------------
>

---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send the following message: SET Technet NOMAIL
Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------

ATOM RSS1 RSS2