Nicolas,
Are the shorts consistently on two parallel sides closest to the
conveyor rails. If so, the part and paste are probably sliding to one side
or another on the domed pads that HASL causes. This usually happens during
the soak zone in the oven when the paste becomes less viscous. We have
found (like many other have found) that using a flat surface finish will
significantly reduce shorts on fine pitch compared with using HASL. If you
are at 38 dpmo (I assume for shorts only?) with HASL, I think you are doing
pretty good. To do better than that, you will have to use a flat surface
finish.
Thanks
Ryan Grant
Advanced Technology Engineer
MCMS
(208) 898-1145
[log in to unmask]
> -----Original Message-----
> From: Nicolas Ortiz [SMTP:[log in to unmask]]
> Sent: Monday, February 05, 2001 1:45 PM
> To: [log in to unmask]
> Subject: [TN] QFP144 solder bridging
>
> Currently we are experiencing solder bridging on a 0.5mm pitch, LQFP,
> 144
> leads. I already reviewed the stencil design, screen printer parameters
> and
> reflow profile. Everything is OK. We have HASL boards. Our current process
> outputs 38 dpmo's. My concern is if I reduce more the apertures, I have
> the
> risk to have solder open or insufficient solder, instead of bridging. Does
> anybody has some input? What dpmo's do you have?
>
> --------------------------------------------------------------------------
> -------
> Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt delivery of Technet send the following message: SET
> Technet NOMAIL
> Search previous postings at: www.ipc.org > On-Line Resources & Databases >
> E-mail Archives
> Please visit IPC web site (http://www.ipc.org/html/forum.htm) for
> additional
> information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
> ext.5315
> --------------------------------------------------------------------------
> -------
---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send the following message: SET Technet NOMAIL
Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------
|
|
|