Hi Jim! Tin and Lead oxides are only marginally conductive. Tin
preferentially oxidizes and is the controlling oxidation reaction for a
tin/lead surface - I have conducted some neat trials to force the reaction
the other direction by using hydrogen peroxide as a treatment solution.
Using the SERA equipment you can literally watch the Sn oxidation
"override" the Pb oxide reactions in a matter of minutes. Take a look at
Chapter Six Oxidation of Solder Coatings in The Mechanics of Solder Alloy
Wetting & Spreading book (ISBN# 0-442-01752-9) for more info. Good Luck.
Dave Hillman
Rockwell Collins
[log in to unmask]
"Marsico, James" <[log in to unmask]>@IPC.ORG> on 01/26/2001 08:09:04
AM
Please respond to "TechNet E-Mail Forum." <[log in to unmask]>; Please respond
to "Marsico, James" <[log in to unmask]>
Sent by: TechNet <[log in to unmask]>
To: [log in to unmask]
cc:
Subject: Re: [TN] silver epoxy & solder coated parts
Thanks for all the responses regarding the use of silver epoxy and solder
coated parts... obviously, not the way to go!
I'm still trying to understand the mechanism for increased DC resistance,
though. From what I have learned, silver oxides are conductive, so this
isn't it. The tin seems to migrate into the epoxy, I assume leaving a
lead-rich zone. Is it that the lead oxidizes? Are lead oxides conductive?
Can anyone explain?
Thanks again,
Jim Marsico
EDO Electronic Systems Group
[log in to unmask] <mailto:[log in to unmask]>
-----Original Message-----
From: Mike Fenner [SMTP:[log in to unmask]]
Sent: Wednesday, January 24, 2001 1:52 PM
To: TechNet E-Mail Forum.; Marsico, James
Subject: Re: [TN] silver epoxy & solder coated parts
I would avoid it.
Conventionally:
Epoxy has poor adhesion to tin and its alloys
The tin/silver interface will give an inter-reaction at the
bondline
leading to electrical opens although you may retain mechanical
adhesion. One/Two years is a long time in this situation especially
if
you have mechanical stress/vibration or any temperature swings in
service.
This is very well documented in the literature and you should see
something in the Technet archives.
More open mindedly:
There are some companies working on this and there are now products
which claim to have solved this problem, either by using a sort of
halfway house product (adhesive with a fusible metal filler
basically)
or by special undisclosed ingredients/formulations.
Contact suppliers for the latest
Mike
----- Original Message -----
From: "Marsico, James" <[log in to unmask]>
To: <[log in to unmask]>
Sent: Tuesday, January 23, 2001 8:34 PM
Subject: [TN] silver epoxy & solder coated parts
> Hello, Technet...
>
> Here is an unusual situation. We have to assemble a surface
mount
assembly
> using silver epoxy. Some of the components will be solder
coated.
I know,
> don't bother asking... this is the way it has to be. The good
thing
is that
> this assembly is a prototype for bench-top laboratory use only.
There is no
> harsh environment and needs to operate 1, maybe 2, years. The
question is
> does anyone foresee any problems? What happens when one mixes
toe
two
> technologies?
>
> Thanks,
> Jim Marsico
> EDO Electronic Systems Group
> [log in to unmask] <mailto:[log in to unmask]>
>
---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send the following message: SET
Technet NOMAIL
Search previous postings at: www.ipc.org > On-Line Resources & Databases >
E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for
additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
---------------------------------------------------------------------------------
---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send the following message: SET Technet NOMAIL
Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------
|