Charles,
For Circuit Pack Assembly it is true than several Lucent manufacturing
locations are using IAg as the surface finish of choice. It has performed
extremely well for us since 1997. However, that doesn't mean IAg is our
solution to the ENi/IAu brittle fracture problem. We, like many others, are
trying to determine the root cause of the problem so that we can determine
when it will happen. We're working on the problem not because we use lots
of ENi/IAu as a surface finish on our circuit packs but because many
companies who sell us packed IC still use ENi/IAu as a surface finish in
their packages. We believe that packagers will probably be using ENi/IAu
for IC packages that require wire bonding for some time to come especially
as I/O count increases. Therefore, we need to understand what causes
brittle ENi/IAu fractures. We also believe that many packagers are
beginning to move away, or considering moving away, from ENi/IAu to OSP or
IAg for flip chip BGAs that don't require wire bonding.
Although the analysis of brittle ENi/IAu fractures is involved and
difficult, we believe we've identified a basic failure mode - fracture at an
intermetallic interface. However, recognizing the MOF is only the initial
step. Corrective action can't be taken to resolve these failures until
failure analysis has identified the root cause(s).
Our initial analysis was presented in the Proceeding from the 26th
International Symposium for Testing and Failure Analysis, 12-16 November,
2000, Bellevue, Washington "Case Studies of Brittle Interfacial Failures in
Area Array Solder Interconnections".
Regards,
George
George M. Wenger, DMTS Bell Laboratories Princeton
Supply Network Solutions
PO Box 900, Princeton NJ 08542-0900
Route 569 Carter Rd., Hopewell, NJ 08525
(609)-639-2769 (Office), 3210 (Lab), 2343 (Fax)
[log in to unmask]
-----Original Message-----
From: Charles E. McMahon [mailto:[log in to unmask]]
Sent: Monday, January 22, 2001 11:57 AM
To: [log in to unmask]
Subject: Re: [TN] Increased Phosphorus in Electroless Ni
As you state George, the problem is part of the nature of the chosen
process.
What would you suggest is a strategy to reduce this incidence of increased
P.
As I recall, LUCENT has turned to silver as a surface coating of choice. Is
this their solution for the phosphorus problem?
Charlie McMahon
-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of Wenger, George M
(George)
Sent: Monday, January 22, 2001 11:12 AM
To: [log in to unmask]
Subject: Re: [TN] Increased Phosphorus in Electroless Ni
Bob,
Dick Coyle and I are glad you responded. We've been too busy to put
together a response. You're correct about P increasing at the interface.
Ther are two processes that cause the increase. One is the replacement
nature of the immersion gold process and the other is the sodlering process
that forms a nickel-tin intermetallic. Both of these, immersion and
soldering, contribute to P incrasing at the interface.
Regards,
George
George M. Wenger, DMTS Bell Laboratories Princeton
Supply Network Solutions
PO Box 900, Princeton NJ 08542-0900
Route 569 Carter Rd., Hopewell, NJ 08525
(609)-639-2769 (Office), 3210 (Lab), 2343 (Fax)
[log in to unmask]
-----Original Message-----
From: Ingemar Hernefjord (EMW)
[mailto:[log in to unmask]]
Sent: Monday, January 22, 2001 10:57 AM
To: [log in to unmask]
Subject: Re: [TN] Increased Phosphorus in Electroless Ni
Hi Lucent and Robert,
when Lucent talks the rest of the world listens...
at least me.
I have been reflecting over your wise words, Robert, and it seems all so
clear, but we have still not succeeded to prove what the mystic, brittle,
unpredictable, invisible and crazy thin layer is really. I have sent a
couple of pictures to big guru himself (W) and can give you one or two also,
because you added worthful words.Otherwise we are restrictive.
Still scratching my own and other's heads
Ingemar
-----Original Message-----
From: Furrow, Robert Gordon (Bob) [mailto:[log in to unmask]]
Sent: den 6 september 2000 22:22
To: 'TechNet E-Mail Forum.'; 'Ingemar Hernefjord (EMW)'
Subject: RE: [TN] Increased Phosphorus in Electroless Ni
I have heard rumblings on several occasions regarding high P% causing
brittle intermetalic failures at the nickel / solder interface. I guess I
just wanted to ask this as a sanity check to see if I am comprehending the
immersion process correctly. If the nickel layer is codeposited in an
electroless process with say 6% to 9% of phosphorus, wouldn't the nickel
layer nearest the solder joint show a higher concentration of P relative to
nickel? I say this based on the immersion gold process, where one atom of
nickel goes into solution as one atom of gold replaces it. Wouldn't this
mean at the gold / nickel interface that there are just a many atoms of P
still present whereas a substantial amount of nickel has been replaced by
gold. When soldering is accomplished, the gold dissolves into the bulk
solder joint and the reduced amount of nickel is left around the original
number of P atoms. If analyzed, the thin interfacial layer of nickel (less
than 10 microinches) would have a high P content relative to the underlying
nickel. Isn't this a natural consequence of the immersion gold process and
to be expected? If so, isn't it more correct to say all soldered connections
near the nickel / solder interface are expected to have an elevated P
content relative to the bulk nickel rather than a thin high P% layer caused
a "black pad" brittle fracture,.
Thanks,
Robert Furrow
SMT Process Engineer
Lucent Technologies
978-960-3224 [log in to unmask]
> -----Original Message-----
> From: Ingemar Hernefjord (EMW) [SMTP:[log in to unmask]]
> Sent: Tuesday, September 05, 2000 11:28 AM
> To: [log in to unmask]
> Subject: Re: [TN] Increased Phosphorus in Electroless Ni
>
> Have little time to read TN nowadays, sorry for that, have to erase most
> before reading, but this one gripped me, because our process engineers
> have just got nervous attacks caused by BGA-soldering problems (double
> sided with 100-600 I/O PBGAs)on FR4 boards, electrical and mechanical
> disorder that is under investigation just now. Small project, fortunately,
> not the large numbers like in our telecom fabs, anyway, one issue that
> came up was the high P% of the electroless Ni, from 7 up to 12%. During
> the up/down ramp for normal soldering intermetallics will be created,
> which is normal, but you may also get a strange interface layer between
> this tin-nickel and the nickel barrier itself, superthin, strange,
> unpredictable layer, hardly visible even in high magnification, can cause
> severe disrupture from CTE-mismatch or other impact. Some of our
> metalurgist say this is connected with too high a P% in Nickel. When other
> baths were used, with much lower P, the problems disappeared. T!
> hat is why I'm interested in what other experiences may come up.
>
> Ingemar Hernefjord
> Ericsson Microwave Systems
>
> -----Original Message-----
> From: Meschter, Stephan J [mailto:[log in to unmask]]
> Sent: den 5 september 2000 15:02
> To: [log in to unmask]
> Subject: [TN] Increased Phosphorus in Electroless Ni
>
>
> Hi:
> We are presently using electroless Ni/Immersion gold metallization
> on our SMT PWBs. Our present requirements are:
> > A. FINAL FINISH TO BE IMMERSION GOLD PLATING, 10 MICRO
> INCHES
> > THICK
> > MAXIMUM, OVER 6-9% PHOSPHORUS CONTAINING ELECTROLESS
> > NICKEL PLATED
> > BASE 0.0003 TO 0.0007 INCHES THICK OVER ELECTRO
> > DEPOSITED COPPER.
> >
> One of our PWB suppliers intends to change their Electroless Nickel bath.
> The current
> phosphorous content of plated nickel is between 6% and 9%. The new bath
> will
> produce phosphorous content between 9% and 12%.
>
> Reason: The higher phosphorous content prevents occurrences of
> "black pad nickel" and also better resist excessive attack on the nickel
> by
> Immersion Gold. So we expect to reduce, or even eliminate, rejections of
> product due to excessive gold or for black nickel under gold.
>
> Does the increased phosphorous content eliminate black pad nickel?
> Is there going to be an effect on solderability or long term solder joint
> life?
> Will the PTH barrel become stronger and result in increased stress in the
> connections between the inner plane and the PTH?
>
> We are concerned that we may be trading one set of problems for another.
>
> Thanks in advance for any help you can offer.
>
>
>
>
> Steph
>
> Stephan Meschter [log in to unmask]
> Lockheed Martin Control Systems Phone :(607)770-2332
> 600 Main Street, MD R52F FAX :(607)770-2056
> Johnson City, NY 13790-1888 MARCALL: 8 * 255-2332
>
> ##############################################################
> TechNet Mail List provided as a free service by IPC using LISTSERV 1.8d
> ##############################################################
> To subscribe/unsubscribe, send a message to [log in to unmask] with
> following text in
> the body:
> To subscribe: SUBSCRIBE TECHNET <your full name>
> To unsubscribe: SIGNOFF TECHNET
> ##############################################################
> Please visit IPC web site (http://www.ipc.org/html/forum.htm) for
> additional
> information.
> If you need assistance - contact Keach Sasamori at [log in to unmask] or
> 847-509-9700 ext.5315
> ##############################################################
>
> ##############################################################
> TechNet Mail List provided as a free service by IPC using LISTSERV 1.8d
> ##############################################################
> To subscribe/unsubscribe, send a message to [log in to unmask] with
> following text in
> the body:
> To subscribe: SUBSCRIBE TECHNET <your full name>
> To unsubscribe: SIGNOFF TECHNET
> ##############################################################
> Please visit IPC web site (http://www.ipc.org/html/forum.htm) for
> additional
> information.
> If you need assistance - contact Keach Sasamori at [log in to unmask] or
> 847-509-9700 ext.5315
> ##############################################################
----------------------------------------------------------------------------
-----
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send the following message: SET
Technet NOMAIL
Search previous postings at: www.ipc.org > On-Line Resources & Databases >
E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
----------------------------------------------------------------------------
-----
----------------------------------------------------------------------------
-----
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send the following message: SET
Technet NOMAIL
Search previous postings at: www.ipc.org > On-Line Resources & Databases >
E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
----------------------------------------------------------------------------
-----
----------------------------------------------------------------------------
-----
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send the following message: SET
Technet NOMAIL
Search previous postings at: www.ipc.org > On-Line Resources & Databases >
E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
----------------------------------------------------------------------------
-----
---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send the following message: SET Technet NOMAIL
Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------
|