Hi Mark,
Below Tg the CTE(x,y)=17+/-2 ppm/C with CTE(x) and CTE(y) differing by about
1 to 2 ppm/C; CTE(z)=50 to 85 ppm/C, depending primarily on resin content.
Above Tg CTE(x,y) may actually drop slightly; CTE(z)=240 to 390 ppm/C, again
depending primarily on resin content. Measuring the CTE(z) over a temperature
range that straddles Tg is nonsense, because you get some mixture of the
respective CTEs below and above Tg that is dependent on the position of Tg
within that rather arbitrary measurment range.
Werner Engelmaier
Engelmaier Associates, L.C.
Electronic Packaging, Interconnection and Reliability Consulting
7 Jasmine Run
Ormond Beach, FL 32174 USA
Phone: 904-437-8747, Fax: 904-437-8737
E-mail: [log in to unmask], Website: www.engelmaier.com
---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send the following message: SET Technet NOMAIL
Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------
|
|
|