Bob-
For what its worth, I've seen this same problem with 2 scenarios:
1. Lack of fluxing action in the paste caused by long hot ramp or long ambient exposure combined with reduced part or pad solderability.
2. Tiny amounts of contaminant (residual conformal coat or adhesive) on pads "floats" to surface of paste during reflow, an instant before the pad solder joins with ball solder.
> Larry Jindra
> TRW/Avionics Systems Division
> mailto:[log in to unmask] ph (858) 592-3424 fax (858) 592-3606
-----Original Message-----
From: bbarr [mailto:[log in to unmask]]
Sent: Wednesday, November 15, 2000 6:45 AM
To: [log in to unmask]
Subject: [TN] BGA Soldering Problem
I have a PBGA357 that is exhibiting a strange (to me) soldering condition.
Two to three balls (not necessarily adjacent, but usually along an edge) do
not appear to be wetting to the solder paste on the land. This is what it
looks like after reflow: The paste on the land has reflowed to a mound, the
ball on the BGA is compressed in shape but not wetted to the mound on the
land (so the ball must have reached reflow temperature to get compressed.) A
clear line of demarcation between the compressed ball and the mound of
solder on the land is visible. The component fails in test, but sometimes
pressing on it can get it to work. In most cases the balls on either side of
the one not wetted look fine. Process is OA flux with convection reflow.
Profile run several months ago with thermocouples imbedded in one center
ball and one edge ball showed max. temp. of 217 (center) and 220 (edge)
degrees C with time above 183 of 56 seconds. Max slope is 2 (center) and 2.8
(edge) degrees C. I am going to go run a verification profile, but in the
mean time your thoughts are much appreciated.
Bob
Robert Barr
Manufacturing Engineering
Formation, Inc.
Voice: 856-234-5020 x3035
Fax: 856-234-6679
email: [log in to unmask]
---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------
---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------
|
|
|