Scott,
First, one must know what bonding technology the Customer is using. Is it
ultrasonic aluminum of thermosonic gold?
If it is aluminum, then the gold is effectively only there to protect the
nickel - to provide a good, clean, nickel surface to bond to (with the 3-5
uinches of gold efectively excluded from the bond). The exception being if
someone has put hard gold on the surface, then it may have been better to
leave the gold off altogether.
If the application is thermosonic gold (where the ultimate goal is a gold to
gold bond), then PURE, SOFT gold of a MINIMUMm of 10-15 uinches is normally
required. If the board is scheduled to see multiple bakes, or elevated temp
storage prior to wirebonding, increases in gold plating thickness are very
helpful. I believe the KEY critical parameter here is PURE gold - such
elements as thallium, cobalt, copper, etc co-deposited in the gold plating
as grain refiners, etc. can extremely quickly ruin a bondable surface. A
'pore free' plated film, if there actually is such a creature, also
facilitates the long term preservation of the plated surface, and its
subsequent bondability.
There have been many other posts concerning adhesive resin bleen, solder
mask bleed-out etc. Naturally, these also may have an effect.
Possibly, some of the more 'plating inclined' individuals out there can add
a few comments. From a User's perspective, if you can find and nurture a
good plater, your life becomes tremendously more forgiving.
Steve Creswick - CTS RF Integrated Modules
##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8d
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in
the body:
To subscribe: SUBSCRIBE TECHNET <your full name>
To unsubscribe: SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information.
If you need assistance - contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
##############################################################
|