a-Tin, commonly known as grey-tin or tin-pest is an allotropic form
of tin. Researchers have found that tin can change form at low temperatures
and become a powdery wartlike structure. The powder has no strength and is
a pure form of tin crystal.
Tin plate or tin lead solder requires an inoculation with a-Tin to initiate
the transformation. However, once started, a-Tin will continue to grow,
completely consuming a joint. One researcher suggest small amounts of
antimony or bismuth will prevent the nucleation of a-Tin.5
5. Phillip E. Hinton, "Tin-Plating, Tin-Nickel Electroplate and Tin-Plating
over Nickel as Final Finishes on Copper", SMI 1996, p807.
Given the above statement, it is unlikely that the white powder you saw is
a-Tin. But if there were no chemicals involved at that site, it is
something that makes you go hmm.
Thanks
Ryan Grant
Advanced Technology Engineer
MCMS
(208) 898-1145
[log in to unmask]
> -----Original Message-----
> From: Hollandsworth, Ron [SMTP:[log in to unmask]]
> Sent: Friday, August 04, 2000 6:27 AM
> To: [log in to unmask]
> Subject: Re: [TN] Alpha Tin
>
> Ryan:
> Refresh my memory on Alpha Tin, if you would please.
>
> Ron
>
> ************************************
> If this email is not intended for you, or you are not responsible for the
> delivery of this message to the addressee, please note that this message
> may
> contain ITT Privileged/Proprietary Information. In such a case, you may
> not
> copy or deliver this message to anyone. You should destroy this message
> and
> kindly notify the sender by reply email. Information contained in this
> message that does not relate to the business of ITT is neither endorsed by
> nor attributable to ITT.
> ************************************
>
> ##############################################################
> TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
> ##############################################################
> To subscribe/unsubscribe, send a message to [log in to unmask] with
> following text in
> the body:
> To subscribe: SUBSCRIBE TECHNET <your full name>
> To unsubscribe: SIGNOFF TECHNET
> ##############################################################
> Please visit IPC web site (http://www.ipc.org/html/forum.htm) for
> additional
> information.
> If you need assistance - contact Keach Sasamori at [log in to unmask] or
> 847-509-9700 ext.5315
> ##############################################################
##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in
the body:
To subscribe: SUBSCRIBE TECHNET <your full name>
To unsubscribe: SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information.
If you need assistance - contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
##############################################################
|