Actually a hole that is "a bit" rough is NOT a bad thing, it provides better
adhesion of the copper plating. A wall that is too smooth is usually covered
with burned and melted epoxy-fiberglass, leaving a surface that has little
affinity for subsequent process.
Desmear leaves a smoother surface then etchback and is in most cases
prefered here at CAE. Etchback usually increasesd wicking and makes the wall
rougher.
Sorry, but I don't have another specification to offer.
All things in moderation may not be a bad thing if you think about it.
Alain Savard, B. Sc.
Chemical Process Analyst
CAE Electronics Ltd.
-----Original Message-----
From: Charles E. McMahon [mailto:[log in to unmask]]
Sent: August 3, 2000 7:48 AM
To: TechNet E-Mail Forum.; Alain Savard
Subject: RE: [TN] Hole wall roughness
As a follow on to your comment Alain to hole wall roughness.
I have seen customers reject boards for hole wall roughness. Using desmear
for cleaning after drill leaves a jagged surface of glass fibers when seen
in cross-section. Plating to it is fine but it put doubts of hole wall
strength in the customers view.
As there are no IPC Standards for determining the roughness of a hole wall,
can a customer reject a board simply based on a unilateral perception that
the hole "looks rough".
Is there a specification outside of IPC that is available for this issue.
Would appreciate your thoughts.
Charles McMahon
-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of Alain Savard
Sent: Thursday, August 03, 2000 7:09 AM
To: [log in to unmask]
Subject: Re: [TN] Hole wall roughness
You could always verify for drilled hole diameter, wicking and nodules with
a microsection. Of course this works best after plating and can be inspected
as per IPC-6012 and IPC-600. You will also get a general idea of the
roughness just by looking at it still on a microsection, this can be checked
on the section prior to plating, but there are no IPC standards for it.
P.S. Wicking is best seen on a non-metallographic microscope wit a good
depth of field.
Alain Savard, B.Sc.
Chemical Process Analyst
CAE Electronics Ltd.
e-mail: [log in to unmask]
-----Original Message-----
From: Shirley Xiao [mailto:[log in to unmask]]
Sent: August 3, 2000 5:32 AM
To: [log in to unmask]
Subject: [TN] Hole wall roughness
Is there anyone knows how to measure hole wall
roughness after drilling or after plating? (Notes:I've
searched TechNet archive but there is nothing about
hole wall roughness.)
Shirley
##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in
the body:
To subscribe: SUBSCRIBE TECHNET <your full name>
To unsubscribe: SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information.
If you need assistance - contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
##############################################################
|
|
|