Steve -
Good lookin' mess - my first suspicion is organics on the board surface at
the t ime of LPI application; second suspicion is too hot/fast a cure
process, skinning the mask before it could expel its volatiles. Regardless,
the problem appears to belong to the fab house at this stage.
Regards - Kelly
-----Original Message-----
From: Stephen R. Gregory <[log in to unmask]>
To: [log in to unmask] <[log in to unmask]>
Date: Wednesday, July 26, 2000 2:17 PM
Subject: [TN] "Bubbly Soldermask..."
>Hi all!
>
>We just got some boards in at receiving inspection that have thousands of
>little "bubbles" in the soldermask all over the boards...they seem to
>concentrate all along the edges of the features of the board. You can see
>pictures of it at:
>
>http://www.driveway.com/share?sid=e25a88c4.8e904&name=Pictures
>
>One picture is bubblemask.jpg, the other is bubblemask2.jpg...what would
>cause that? It's a LPI...don't know the brand name. I'm thinking that
either
>the boards weren't dry or cleaned well prior to soldermasking them. I'm
>rejecting the boards of course...
>
>My freedrive is filling up fast with all the pictures of the "pretty
boards"
>that we get from our vendors!!!
>
>-Steve Gregory-
>
>##############################################################
>TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
>##############################################################
>To subscribe/unsubscribe, send a message to [log in to unmask] with following
text in
>the body:
>To subscribe: SUBSCRIBE TECHNET <your full name>
>To unsubscribe: SIGNOFF TECHNET
>##############################################################
>Please visit IPC web site (http://www.ipc.org/html/forum.htm) for
additional
>information.
>If you need assistance - contact Keach Sasamori at [log in to unmask] or
>847-509-9700 ext.5315
>##############################################################
##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in
the body:
To subscribe: SUBSCRIBE TECHNET <your full name>
To unsubscribe: SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information.
If you need assistance - contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
##############################################################
|
|
|